# US 2003/0067003 A1 · Tin oxide nanostructures

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2003/0067003 A1
- Document ID: US20030067003A1
- Status: Published application
- Kind: A1
- Application number: 10/261,149
- Filed: 2002-09-30
- Published: 2003-04-10
- Earliest claimed: 2001-09-28
- Assignees: Georgia Tech Research Corporation
- Inventors: James L. Gole; Z.L. Wang
- Web page: https://patentgrep.com/patent/US20030067003A1

## CPC

- H10D 62/118: {Nanostructure semiconductor bodies}
- B82Y 10/00: Nanotechnology for information processing, storage or transmission, e.g. quantum computing or single electron logic
- B82Y 30/00: Nanotechnology for materials or surface science, e.g. nanocomposites
- H10D 62/119: {Nanowire, nanosheet or nanotube semiconductor bodies}
- H10D 62/121: {oriented parallel to substrates}
- Y10S 977/762: Nanowire or quantum wire, i.e. axially elongated structure having two dimensions of 100 nm or less
- H10D: INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
- B82Y: SPECIFIC USES OR APPLICATIONS OF NANOSTRUCTURES; MEASUREMENT OR ANALYSIS OF NANOSTRUCTURES; MANUFACTURE OR TREATMENT OF NANOSTRUCTURES
- Y10S: TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS

## Abstract

Tin oxide nanostructures and methods of fabricating tin oxide nanostructures are disclosed. Representative nanostructures include SnO2 nanowires, SnO2 nanoribbons, and SnO2 nanotubes. Another representative nanostructure includes a nanostructure having a rutile crystal lattice and an orthorhombic crystal superlattice. The nanostructure can include, but is not limited to, SnO2 nanowires, SnO2 nanoribbons, and SnO2 nanotubes.

## Claims

### Claim 1

A nanostructure, comprising a tin oxide (SnO2) nanowire.

### Claim 2 (depends on 1)

The nanostructure of claim 1, wherein the SnO2 nanowire has a rutile crystal structure.

### Claim 3 (depends on 1)

The nanostructure of claim 1, wherein the SnO2 nanowire is substantially circular.

### Claim 4 (depends on 1)

The nanostructure of claim 1, wherein the SnO2 nanowire is substantially rectangular.

### Claim 5 (depends on 1)

The nanostructure of claim 1, wherein the SnO2 nanowire has a rectangular cross section enclosed by ±(010) and ±(10{overscore (1)}) facet planes, and wherein the growth direction is parallel the [101] crystal direction.

### Claim 6 (depends on 1)

The nanostructure of claim 1, wherein the SnO2 nanowire has a thickness-to-width aspect ratio ranging from about 1:2 to about 1:5.

### Claim 7 (depends on 1)

The nanostructure of claim 1, wherein the SnO2 nanowire has a diameter between about 10 nanometers to 100 nanometers.

### Claim 8 (depends on 1)

The nanostructure of claim 1, wherein the SnO2 nanowire has a length between about 10 micrometers to 300 micrometers.

### Claim 9

A nanostructure, comprising a tin oxide (SnO2) nanowire having a rutile crystal lattice and an orthorhombic crystal superlattice.

### Claim 10 (depends on 9)

The nanostructure of claim 9, wherein the SnO2 nanowire has a rectangular cross-section and is enclosed by ±(100)o/±(010)t and ±(001)o/±(10{overscore (1)})t facet planes and a growth direction along the [010]o crystal direction that is parallel to [101]t of the SnO2 rutile crystal lattice.

### Claim 11 (depends on 9)

The nanostructure of claim 9, wherein the orientation relationship between the orthorhombic SnO2 supperlattice and the rutile SnO2 crystal lattice of the SnO2 nanowire corresponds to [001]o∥[10{overscore (2)}]t and (100)o∥(010)t.

### Claim 12 (depends on 9)

The nanostructure of claim 9, wherein the SnO2 nanowire is substantially circular.

### Claim 13 (depends on 9)

The nanostructure of claim 9, wherein the SnO2 nanowire is substantially rectangular.

### Claim 14 (depends on 9)

The nanostructure of claim 9, wherein the SnO2 nanowire has a diameter between about 10 nanometers to 100 nanometers.

### Claim 15 (depends on 9)

The nanostructure of claim 9, wherein the SnO2 nanowire has a length between about 10 micrometers to 300 micrometers.

### Claim 16

A nanostructure, comprising a tin oxide (SnO2) sandwiched nanoribbon.

### Claim 17 (depends on 16)

The nanostructure of claim 16, wherein the SnO2 sandwiched nanoribbon has a rutile crystal lattice and an orthorhombic crystal superlattice.

### Claim 18 (depends on 16)

The nanostructure of claim 16, wherein the orientation relationship between the orthorhombic SnO2 supperlattice and the rutile SnO2 crystal lattice of the SnO2 sandwiched nanoribbon corresponds to [001]o∥[10{overscore (2)}]t and (100)o∥(010)t.

### Claim 19 (depends on 16)

The nanostructure of claim 16, wherein the SnO2 sandwiched nanoribbon is enclosed by ±(110)o/±(231)t and ±(001)o/±(10{overscore (1)})t facet planes, and wherein the growth directions are parallel to [110]o/[111]t.

### Claim 20 (depends on 16)

The nanostructure of claim 16, wherein the SnO2 sandwiched nanoribbon has a first side thickness of about 20 nanometers, a second side thickness of about 20 nanometers, and a core layer width of about 120 nanometers.

### Claim 21 (depends on 16)

The nanostructure of claim 16, wherein the SnO2 sandwiched nanoribbon has a length between about 10 micrometers to 300 micrometers.

### Claim 22

A nanostructure, comprising a tin oxide (SnO2) nanotube.

### Claim 23 (depends on 22)

The nanostructure of claim 22, wherein the SnO2 nanotube has a rutile crystal lattice and an orthorhombic crystal superlattice.

### Claim 24 (depends on 22)

The nanostructure of claim 22, wherein the SnO2 nanotube is substantially hollow.

### Claim 25 (depends on 22)

The nanostructure of claim 22, wherein the SnO2 nanotube has a growth direction parallel to [{overscore (1)}10]o with respect to the orthorhombic SnO2 superlattice.

### Claim 26 (depends on 22)

The nanostructure of claim 22, wherein the SnO2 nanotube has a diameter of between about 50 nanometers and 350 nanometers and a length of about 3 to about 5 micrometers.

### Claim 27 (depends on 22)

The nanostructure of claim 22, wherein the orientation relationship between the orthorhombic SnO2 supperlattice and the rutile SnO2 crystal lattice of the SnO2 nanotube corresponds to [001]o∥[3{overscore (17)}]t and ±(110)o∥(451)t.

### Claim 28

A structure, comprising a nanostructure having a rutile crystal lattice and an orthorhombic crystal superlattice.

### Claim 29 (depends on 28)

The structure of claim 28, wherein the nanostructure is selected from a SnO2 nanowire, a SnO2 nanoribbon, a SnO2 nanotube.

### Claim 30

A method of forming an SnO2 nanostructure, comprising:
forming a plurality of layers of tin (Sn) and tin oxide (SnO); and
heating the plurality of layers to between about 1000° C. and 1200° C. for between about 3 and 12 hours at a pressure of between about 150 Torr and 750 Torr.

### Claim 31

A method of forming a nanostructure, comprising:
providing an oxygen lean environment by alternating layers of tin (Sn) and tin oxide (SnO);
heating the plurality of layers to between about 1000° C. and 1200° C. for between about 3 and 12 hours at a pressure of between about 150 Torr and 750 Torr; and
forming an SnO2 nanostructure.

### Claim 32

A method of forming a nanostructure, comprising:
providing tin oxide (SnO) powder in an oxygen lean environment;
heating the SnO powder to between about 1000° C. and 1200° C. for between about 3 and 12 hours at a pressure of between about 150 Torr and 750 Torr; and
forming an SnO2 nanostructure.