# US 2003/0037847 A1 · High purity tantalum, products containing the same, and methods of making the same

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2003/0037847 A1
- Document ID: US20030037847A1
- Status: Published application
- Kind: A1
- Application number: 10/145,336
- Filed: 2002-05-14
- Published: 2003-02-27
- Earliest claimed: 1998-11-25
- Assignees: Cabot Corporation
- Inventors: Christopher A. Michaluk; Louis E. Huber; Mark N. Kawchak; James D. Maguire JR.
- Web page: https://patentgrep.com/patent/US20030037847A1

## CPC

- C23C 14/3414: {Metallurgical or chemical aspects of target preparation, e.g. casting, powder metallurgy}
- C22B 34/24: Obtaining niobium or tantalum
- Y10S 148/014: Capacitor
- Y10S 148/158: Sputtering
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- C22B: PRODUCTION AND REFINING OF METALS (electrolytic C25); PRETREATMENT OF RAW MATERIALS
- Y10S: TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS

## Abstract

High purity tantalum metals and alloys containing the same are described. The tantalum metal preferably has a purity of at least 99.995% and more preferably at least 99.999%. In addition, tantalum metal and alloys thereof are described, which either have a grain size of about 50 microns or less, or a texture in which a (100) intensity within any 5% increment of thickness is less than about 15 random, or an incremental log ratio of (111):(100) intensity of greater than about −4.0, or any combination of these properties. Also described are articles and components made from the tantalum metal which include, but are not limited to, sputtering targets, capacitor cans, resistive film layers, wire, and the like. Also disclosed is a process for making the high purity metal which includes the step of reacting a salt-containing tantalum with at least one compound capable of reducing this salt to tantalum powder and a second salt in a reaction container. The reaction container or liner in the reaction container and the agitator or liner on the agitator are made from a metal material having the same or higher vapor pressure of melted tantalum. The high purity tantalum preferably has a fine and uniform microstructure.

## Claims

### Claim 1

Tantalum metal having a purity of at least about 99.995%, and an average grain size of about 150 microns or less.

### Claim 2 (depends on 1)

The tantalum metal of claim 1, wherein said metal is fully recrystallized.

### Claim 3 (depends on 1)

The tantalum metal of claim 1, wherein said metal is at least partially recrystallyzed.

### Claim 4 (depends on 1)

The tantalum metal of claim 1, wherein about 98% or more of said metal is recrystallyzed.

### Claim 5 (depends on 1)

The tantalum metal of claim 1, wherein about 80% or more of said metal is recrystallyzed.

### Claim 6 (depends on 1)

The tantalum metal of claim 1, wherein said metal has a) a texture in which a (100) pole figure has a center peak intensity less than about 15 random or b) a log ratio of (111):(100) center peak intensities of greater than about −4.0, or c) both.

### Claim 7 (depends on 6)

The tantalum metal of claim 6, wherein said center peak intensity is from about 0 random to about 15 random.

### Claim 8 (depends on 6)

The tantalum metal of claim 6, wherein said center peak intensity is from about 0 random to about 10 random.

### Claim 9 (depends on 6)

The tantalum metal of claim 6, wherein said log ratio is from about −4.0 to about 15.

### Claim 10 (depends on 6)

The tantalum metal of claim 6, wherein said log ratio is from about −1.5 to about 7.0.

### Claim 11 (depends on 6)

The tantalum metal of claim 6, wherein said center peak intensity is from about 0 random to about 15 random, and said log ratio is from about −4.0 to about 15.

### Claim 12 (depends on 1)

The tantalum metal of claim 1 having a purity of from 99.995% to about 99.999%.

### Claim 13 (depends on 1)

A metal alloy comprising the tantalum metal of claim 1.

### Claim 14 (depends on 6)

A metal alloy comprising the tantalum metal of claim 6.

### Claim 15 (depends on 3)

A metal alloy comprising the tantalum metal of claim 3.

### Claim 16 (depends on 1)

A sputtering target comprising the tantalum metal of claim 1.

### Claim 17 (depends on 6)

A sputtering target comprising the tantalum metal of claim 6.

### Claim 18 (depends on 3)

A sputtering target comprising the tantalum metal of claim 3.

### Claim 19 (depends on 1)

A capacitor can comprising the tantalum metal of claim 1.

### Claim 20 (depends on 6)

A capacitor can comprising the tantalum metal of claim 6.

### Claim 21 (depends on 3)

A capacitor can comprising the tantalum metal of claim 3.

### Claim 22 (depends on 1)

A resistive film layer comprising the tantalum metal of claim 1.

### Claim 23 (depends on 6)

A resistive film layer comprising the tantalum metal of claim 6.

### Claim 24 (depends on 3)

A resistive film layer comprising the tantalum metal of claim 3.

### Claim 25 (depends on 1)

An article comprising at least as a component the tantalum metal of claim 1.

### Claim 26 (depends on 6)

An article comprising at least as a component the tantalum metal of claim 6.

### Claim 27 (depends on 3)

An article comprising at least as a component the tantalum metal of claim 3.

### Claim 28

Tantalum metal having a) an average grain size of about 50 microns or less, or b) a texture in which a (100) pole figure has a center peak intensity equal to or less than about 15 random or c) a log ratio of (111):(100) center peak intensities of greater than about −4.0, or combinations thereof.

### Claim 29 (depends on 28)

The tantalum metal of claim 28 having an average grain size of from about 25 to about 50 microns.

### Claim 30 (depends on 28)

The tantalum metal of claim 28 having a ratio of (111):(100) center peak intensities of greater than about −4.0.

### Claim 31 (depends on 28)

The tantalum metal of claim 28, having both a) and b).

### Claim 32 (depends on 28)

The tantalum metal of claim 28, wherein said metal has purity of at least 99.995% tantalum.

### Claim 33 (depends on 28)

The tantalum metal of claim 28, wherein said metal has a purity of 99.999% tantalum.

### Claim 34 (depends on 28)

The tantalum metal of claim 28, wherein said metal is fully recrystallized.

### Claim 35 (depends on 32)

The tantalum metal of claim 32, wherein said metal is fully recrystallized.

### Claim 36 (depends on 33)

The tantalum metal of claim 33, wherein said metal is fully recrystallized.

### Claim 37 (depends on 28)

The tantalum metal of claim 28, wherein about 80% or more of said metal is fully recrystallized.

### Claim 38 (depends on 28)

The tantalum metal of claim 28, wherein said center peak intensity is from about 0 random to about 15 random.

### Claim 39 (depends on 28)

The tantalum metal of claim 28, wherein said log ratio is from about −4.0 to about 15.

### Claim 40 (depends on 28)

An article comprising the tantalum metal of claim 28.

### Claim 41 (depends on 33)

An article comprising the tantalum metal of claim 33.

### Claim 42 (depends on 28)

A sputtering target comprising the tantalum metal of claim 28.

### Claim 43 (depends on 33)

A sputtering target comprising the tantalum metal of claim 33.

### Claim 44 (depends on 1)

A process for making the tantalum metal of claim 1, comprising reacting a salt containing tantalum with at least one agent capable of reducing the salt to tantalum and a second salt in a reaction container having an agitator, wherein the reaction container or a liner in the reaction container and the agitator or a liner on the agitator are made from a metal material having the same or higher vapor pressure of tantalum at the melting point of the tantalum.

### Claim 45 (depends on 44)

The process of claim 44, wherein the salt containing tantalum comprises a potassium-fluoride tantalum and the agent comprises sodium.

### Claim 46 (depends on 45)

The process of claim 45, wherein the second salt comprises sodium fluoride and/or sodium chloride.

### Claim 47 (depends on 44)

The process of claim 44, wherein prior to reacting said salt containing tantalum, said process comprising forming an acid solution comprising tantalum and impurities and conducting a density separation of the acid solution containing tantalum from the acid solution containing the impurities; and crystallizing the acid solution containing the tantalum to form the salt containing tantalum.

### Claim 48 (depends on 47)

The process of claim 47, wherein the tantalum and impurities are crushed ore comprising tantalum and impurities.

### Claim 49 (depends on 47)

The process of claim 47, wherein the acid solution comprising tantalum and impurities are formed by combining acid solution with crushed ore comprising tantalum.

### Claim 50 (depends on 44)

The process of claim 44, wherein the reaction occurs at about 800° C. to about 1100° C. while stirring.

### Claim 51 (depends on 44)

The process of claim 44, wherein the reaction container or liner and the agitator or liner on the agitator are metal-based, wherein said metal is nickel, chromium, iron, manganese, titanium, zirconium, hafnium, vanadium, technetium, ruthenium, cobalt, rhodium, palladium, platinum, or any combination thereof.

### Claim 52 (depends on 51)

The process of claim 51, wherein the metal is nickel or a nickel-based alloy.

### Claim 53 (depends on 51)

The process of claim 51, wherein the metal is chromium or a chromium-based alloy.

### Claim 54 (depends on 51)

The process of claim 51, wherein the metal is iron or an iron-based alloy.

### Claim 55 (depends on 44)

The process of claim 44, further comprising recovering tantalum by dissolving the second salt in an aqueous solution.

### Claim 56 (depends on 55)

The process of claim 55, further comprising melting said recovered tantalum in a sufficient vacuum to remove substantially any existing impurities in said recovered tantalum and obtain high purity tantalum.

### Claim 57 (depends on 56)

The process of claim 56, wherein the vacuum is 10−4 torr or more.

### Claim 58 (depends on 56)

The process of claim 56, wherein the pressure above the melted recovered tantalum is lower than the vapor pressures of substantially all of the impurities.

### Claim 59 (depends on 56)

The process of claim 56, wherein the impurities are removed by vaporization of the impurities.

### Claim 60 (depends on 56)

The process of claim 56, wherein said melting is accomplished by electron beam melting.

### Claim 61 (depends on 56)

The process of claim 56, wherein said melting is accomplished by vacuum arc remelt processing.

### Claim 62 (depends on 56)

The process of claim 56, wherein the high purity tantalum is allowed to form a solid and subjected to a rolling process, a forging process, or both.

### Claim 63 (depends on 1)

The tantalum metal of claim 1, wherein the tantalum metal has a substantially fine and uniform microstructure.

### Claim 64 (depends on 1)

The tantalum metal of claim 1, wherein the tantalum metal has an average grain size of from about 25 to about 150 microns.

### Claim 65 (depends on 64)

The tantalum metal of claim 64, wherein the tantalum metal has an average grain size of from about 25 to about 100 microns.

### Claim 66 (depends on 65)

The tantalum metal of claim 65, wherein the tantalum metal has an average grain size of from about 25 to about 75 microns.

### Claim 67

A process of making a sputtering target from tantalum metal having a purity of at least 99.995%, comprising:
a) mechanically or chemically clean surfaces of the tantalum metal, wherein the tantalum metal has a sufficient starting cross-sectional area to permit steps b) through g);
b) flat forging the tantalum metal into at least one rolling slab, wherein the at least one rolling slab has sufficient deformation to achieve substantially uniform recrystallization after annealing in step d);
c) mechanically or chemically clean surfaces of the at least one rolling slab;
d) annealing the at least one rolling slab at a sufficient temperature and for a sufficient time to achieve at least partial recrystallization of the at least one rolling slab;
e) cold or warm rolling the at least one rolling slab in both the perpendicular and parallel directions to the axis of the starting tantalum metal to form at least one plate;
f) flattening the at least one plate; and
g) annealing the at least one plate to have an average grain size equal to or less than about 150 microns and a texture substantially void of (100) textural bands;

### Claim 68 (depends on 67)

The process of claim 67, wherein the tantalum metal has a purity of at least 99.999%.

### Claim 69 (depends on 67)

The process of claim 67, wherein the flat forging occurs after the tantalum metal is placed in air for at least about 4 hours and from temperatures ranging from ambient to about 1200° C.

### Claim 70 (depends on 67)

The process of claim 67, wherein the cold rolling is transverse rolling at ambient temperatures and the warm rolling is at temperatures of less than about 370° C.

### Claim 71 (depends on 67)

The process of claim 67, wherein the annealing of the plate is vacuum annealing at a temperature and for a time sufficient to achieve recrystallization of the tantalum metal.

### Claim 72

A process of making a sputtering target from tantalum metal having a purity of at least 99.995%, comprising:
a) mechanically or chemically clean surfaces of the tantalum metal, wherein the tantalum metal has a sufficient starting cross-sectional area to permit steps b) through i);
b) round forging the tantalum metal into at least one rod, wherein the at least one rod has sufficient deformation to achieve substantially uniform recrystallization after annealing in step d) or step f);
c) cutting the rod into billets and mechanically or chemically clean the surfaces of the billets;
d) optionally annealing the billets to achieve at least partial recrystallization;
e) axially forging billets into preforms;
f) optionally annealing the preforms to achieve at least partial recrystallization;
g) cold rolling the preforms into at least one plate; and
h) optionally mechanically or chemically clean the surfaces of the at least one plate; and
i) annealing the at least one plate to have an average grain size equal to or less than about 150 microns and a texture substantially void of (100) textural bands, wherein annealing occurs at least in step d) or f) or both.

### Claim 73 (depends on 72)

The process of claim 72, wherein the tantalum metal has a purity of at least 99.999%.

### Claim 74 (depends on 72)

The process of claim 72, wherein the round forging occurs after subjecting the tantalum metal to temperatures of about 370° C. or lower.

### Claim 75 (depends on 72)

The process of claim 72 wherein prior to forging the billets, the billets are annealed.

### Claim 76 (depends on 72)

The process of claim 72, wherein prior to cold rolling of the preforms, the preforms are annealed.

### Claim 77 (depends on 72)

The process of claim 72, wherein the annealing of the preforms is vacuum annealing at a sufficient temperature and for a time to achieve recrystallization.

### Claim 78

A tantalum sputtering component comprising an average grain size of about 150 microns or less and a uniform texture of primary (111) throughout a thickness of the component.

### Claim 79 (depends on 78)

The tantalum sputtering component of claim 78, wherein said tantalum sputtering component is a sputtering target.

### Claim 80 (depends on 78)

The tantalum sputtering component of claim 78, wherein said tantalum sputtering component has 50 ppm or less metallic impurities.

### Claim 81 (depends on 78)

The tantalum sputtering component of claim 78, further having 50 ppm or less O2, 25 ppm or less N2, or 25 ppm or less carbon, or combinations thereof.

### Claim 82 (depends on 78)

The tantalum sputtering component of claim 78, having 10 ppm or less metallic impurities.

### Claim 83 (depends on 78)

The tantalum sputtering component of claim 78, further having 50 ppm or less O2, 25 ppm or less N2, or 25 ppm or less carbon, or combinations thereof.

### Claim 84 (depends on 78)

A sputtered deposited film of tantalum produced by the sputtering component of claim 78.

### Claim 85 (depends on 78)

The tantalum sputtering component of claim 78, wherein said average grain size is about 100 microns or less.

### Claim 86 (depends on 85)

The tantalum sputtering component of claim 85, wherein said tantalum sputtering component is a sputtering target.

### Claim 87 (depends on 78)

The tantalum sputtering component of claim 78, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.50% tantalum.

### Claim 88 (depends on 78)

The tantalum sputtering component of claim 78, wherein said tantalum sputtering comprises tantalum having a purity of at least 99.99% tantalum.

### Claim 89 (depends on 78)

The tantalum sputtering component of claim 78, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.995% tantalum.

### Claim 90 (depends on 78)

The tantalum sputtering component of claim 78, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.999% tantalum.

### Claim 91 (depends on 78)

The tantalum sputtering component of claim 78, wherein said tantalum sputtering component is fully recrystallized.

### Claim 92 (depends on 78)

The tantalum sputtering component of claim 78, wherein said tantalum sputtering component is at least partially recrystallized.

### Claim 93 (depends on 78)

The tantalum sputtering component of claim 78, wherein about 98% or more of said tantalum sputtering component is recrystallized.

### Claim 94 (depends on 78)

The tantalum sputtering component of claim 78, wherein about 80% or more of said tantalum sputtering component is recrystallized.

### Claim 95 (depends on 78)

The tantalum sputtering component of claim 78, wherein said tantalum sputtering component has a) a texture in which a (100) pole figure has a center peak intensity less than about 15 random or b) a log ratio of (111):(100) center peak intensities of greater than about −4.0, or c) both.

### Claim 96 (depends on 95)

The tantalum sputtering component of claim 95, wherein said center peak intensity is from about 0 random to less than about 15 random.

### Claim 97 (depends on 95)

The tantalum sputtering component of claim 95, wherein said center peak intensity is from about 0 random to about 10 random.

### Claim 98 (depends on 95)

The tantalum sputtering component of claim 95, wherein said log ratio is from greater than about −4.0 to about 15.

### Claim 99 (depends on 95)

The tantalum sputtering component of claim 95, wherein said log ratio is from about −1.5 to about 7.0.

### Claim 100 (depends on 95)

The tantalum sputtering component of claim 95, wherein said center peak intensity is from about 0 random to less than about 15 random, and said log ratio is from greater than about −4.0 to about 15.

### Claim 101 (depends on 78)

The tantalum sputtering component of claim 78 having a purity of from 99.995% to about 99.999%.

### Claim 102 (depends on 78)

The tantalum sputtering component of claim 78, wherein said average grain size is about 50 microns or less.

### Claim 103 (depends on 78)

The tantalum sputtering component of claim 78, wherein said average grain size is from about 25 to about 150 microns.

### Claim 104 (depends on 85)

The tantalum sputtering component of claim 85, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.50% tantalum.

### Claim 105 (depends on 85)

The tantalum sputtering component of claim 85, wherein said tantalum sputtering comprises tantalum having a purity of at least 99.99% tantalum.

### Claim 106 (depends on 85)

The tantalum sputtering component of claim 85, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.995% tantalum.

### Claim 107 (depends on 85)

The tantalum sputtering component of claim 85, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.999% tantalum.

### Claim 108 (depends on 78)

The tantalum sputtering component of claim 78, wherein said average grain size is about 125 microns or less.

### Claim 109 (depends on 85)

The tantalum sputtering component of claim 85, wherein said tantalum sputtering component is fully recrystallized.

### Claim 110 (depends on 85)

The tantalum sputtering component of claim 85, wherein said tantalum sputtering component is at least partially recrystallized.

### Claim 111 (depends on 85)

The tantalum sputtering component of claim 85, wherein about 98% or more of said tantalum sputtering component is recrystallized.

### Claim 112 (depends on 85)

The tantalum sputtering component of claim 85, wherein about 80% or more of said tantalum sputtering component is recrystallized.

### Claim 113 (depends on 85)

The tantalum sputtering component of claim 85, wherein said tantalum sputtering component has a) a texture in which a (100) pole figure has a center peak intensity less than about 15 random or b) a log ratio of (111):(100) center peak intensities of greater than about −4.0, or c) both.

### Claim 114 (depends on 113)

The tantalum sputtering component of claim 113, wherein said center peak intensity is from about 0 random to less than about 15 random.

### Claim 115 (depends on 113)

The tantalum sputtering component of claim 113, wherein said center peak intensity is from about 0 random to about 10 random.

### Claim 116 (depends on 113)

The tantalum sputtering component of claim 113, wherein said log ratio is from greater than about 4.0 to about 15.

### Claim 117 (depends on 113)

The tantalum sputtering component of claim 113, wherein said log ratio is from about −1.5 to about 7.0.

### Claim 118 (depends on 113)

The tantalum sputtering component of claim 113, wherein said center peak intensity is from about 0 random to less than about 15 random, and said log ratio is from greater than about 4.0 to about 15.

### Claim 119 (depends on 85)

The tantalum sputtering component of claim 85 having a purity of from 99.995% to about 99.999%.

### Claim 120

A tantalum sputtering component comprising a) an average grain size of about 50 microns or less, or b) a texture in which a (100) pole figure has a center peak intensity equal to or less than about 15 random or c) a log ratio of (111):(100) center peak intensities of greater than about −4.0, or combinations thereof.

### Claim 121 (depends on 120)

The tantalum sputtering component of claim 120 having an average grain size of from about 25 to about 50 microns.

### Claim 122 (depends on 120)

The tantalum sputtering component of claim 120, having both a) and b).

### Claim 123 (depends on 120)

The tantalum sputtering component of claim 120, wherein said metal has purity of at least 99.50% tantalum.

### Claim 124 (depends on 120)

The tantalum sputtering component of claim 120, wherein said metal has a purity of at least 99.995% tantalum.

### Claim 125 (depends on 120)

The tantalum sputtering component of claim 120, wherein said metal is fully recrystallized.

### Claim 126 (depends on 120)

The tantalum sputtering component of claim 120, wherein said metal is fully recrystallized.

### Claim 127 (depends on 120)

The tantalum sputtering component of claim 120, wherein said metal is fully recrystallized.

### Claim 128 (depends on 120)

The tantalum sputtering component of claim 120, wherein about 80% or more of said metal is fully recrystallized.

### Claim 129 (depends on 120)

The tantalum sputtering component of claim 120, wherein said center peak intensity is from about 0 random to about 15 random.

### Claim 130 (depends on 120)

The tantalum sputtering component of claim 120, wherein said log ratio is from about 4.0 to about 15.

### Claim 131 (depends on 78)

The sputtering target of claim 78, wherein the tantalum sputtering component has a substantially fine and uniform microstructure.

### Claim 132

A tantalum sputtering component comprising tantalum metal a purity of at least about 99.50%, an average grain size of about 150 microns or less, and having a) a texture in which a (100) pole figure has a center peak intensity less than about 15 random or b) a log ratio of (111):(100) center peak intensities of greater than about 4.0, or c) both.

### Claim 133 (depends on 132)

The tantalum sputtering component of claim 132, wherein said metal is fully recrystallized.

### Claim 134 (depends on 132)

The tantalum sputtering component of claim 132, wherein said metal is at least partially recrystallized.

### Claim 135 (depends on 132)

The tantalum sputtering component of claim 132, wherein about 98% or more of said metal is recrystallized.

### Claim 136 (depends on 132)

The tantalum sputtering component of claim 132, wherein about 80% or more of said metal is recrystallized.

### Claim 137 (depends on 132)

The tantalum sputtering component of claim 132, wherein said center peak intensity is from about 0 random to less than about 15 random.

### Claim 138 (depends on 132)

The tantalum sputtering component of claim 132, wherein said center peak intensity is from about 0 random to about 10 random.

### Claim 139 (depends on 132)

The tantalum sputtering component of claim 132, wherein said log ratio is from greater than about 4.0 to about 15.

### Claim 140 (depends on 132)

The tantalum sputtering component of claim 132, wherein said log ratio is from about −1.5 to about 7.0.

### Claim 141 (depends on 132)

The tantalum sputtering component of claim 132, wherein said center peak intensity is from about 0 random to less than about 15 random, and said log ratio is from greater than about 4.0 to about 15.

### Claim 142 (depends on 132)

The tantalum sputtering component of claim 132, wherein said tantalum sputtering component is a sputtering target

### Claim 143 (depends on 85)

The tantalum sputtering component of claim 85, wherein said tantalum sputtering component has 50 ppm or less metallic impurities.

### Claim 144 (depends on 85)

The tantalum sputtering component of claim 85, further having 50 ppm or less O2, 25 ppm or less N2, or 25 ppm or less carbon, or combinations thereof.

### Claim 145 (depends on 85)

The tantalum sputtering component of claim 85, having 10 ppm or less metallic impurities.

### Claim 146 (depends on 85)

The tantalum sputtering component of claim 85, further having 50 ppm or less O2, 25 ppm or less N2, or 25 ppm or less carbon, or combinations thereof.

### Claim 147 (depends on 85)

A sputtered deposited film of tantalum produced by a sputtering component of claim 85.

### Claim 148

A tantalum sputtering component comprising a uniform texture of primary (111) throughout a thickness of the component.

### Claim 149 (depends on 148)

The tantalum sputtering component of claim 148, wherein said tantalum sputtering component is a sputtering target.

### Claim 150 (depends on 148)

A sputtered deposited film of tantalum produced by a sputtering component of claim 148.

### Claim 151 (depends on 148)

The tantalum sputtering component of claim 148, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.50% tantalum.

### Claim 152 (depends on 148)

The tantalum sputtering component of claim 148, wherein said tantalum sputtering comprises tantalum having a purity of at least 99.99% tantalum.

### Claim 153 (depends on 148)

The tantalum sputtering component of claim 148, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.995% tantalum.

### Claim 154 (depends on 148)

The tantalum sputtering component of claim 148, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.999% tantalum.

### Claim 155 (depends on 148)

The tantalum sputtering component of claim 148, wherein said tantalum sputtering component is fully recrystallized.

### Claim 156

A tantalum sputtering component comprising an average grain size of about 150 microns or less and a uniform texture of mixed (111) throughout its thickness.

### Claim 157 (depends on 156)

The tantalum sputtering component of claim 156, wherein said tantalum sputtering component is a sputtering target.

### Claim 158 (depends on 156)

The tantalum sputtering component of claim 156, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.50% tantalum.

### Claim 159 (depends on 156)

The tantalum sputtering component of claim 156, wherein said tantalum sputtering comprises tantalum having a purity of at least 99.99% tantalum.

### Claim 160 (depends on 156)

The tantalum sputtering component of claim 156, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.995% tantalum.

### Claim 161 (depends on 156)

The tantalum sputtering component of claim 156, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.999% tantalum.

### Claim 162 (depends on 156)

The tantalum sputtering component of claim 156, wherein said tantalum sputtering component is fully recrystallized.

### Claim 163 (depends on 156)

The tantalum sputtering component of claim 156, wherein said tantalum sputtering component is at least partially recrystallized.

### Claim 164 (depends on 156)

The tantalum sputtering component of claim 156, wherein about 98% or more of said tantalum sputtering component is recrystallized.

### Claim 165 (depends on 156)

The tantalum sputtering component of claim 156, wherein about 80% or more of said tantalum sputtering component is recrystallized.

### Claim 166 (depends on 156)

The tantalum sputtering component of claim 156, wherein said grain size is about 100 microns or less.

### Claim 167 (depends on 156)

The tantalum sputtering component of claim 156, wherein said grain size is about 50 microns or less.

### Claim 168 (depends on 156)

The tantalum sputtering component of claim 156, wherein said average grain size is from about 25 to about 150 microns.

### Claim 169

A tantalum sputtering component comprising a primary or mixed (111)-type texture throughout its thickness which is substantially void of (100) textural bands.

### Claim 170 (depends on 169)

The tantalum sputtering component of claim 169, wherein said tantalum sputtering component has an average grain size of about 150 microns or less.

### Claim 171 (depends on 169)

The tantalum sputtering component of claim 169, wherein said average grain size is about 100 microns or less.

### Claim 172 (depends on 169)

The tantalum sputtering component of claim 169, wherein said tantalum sputtering component is a sputtering target.

### Claim 173 (depends on 169)

The tantalum sputtering component of claim 169, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.50% tantalum.

### Claim 174 (depends on 169)

The tantalum sputtering component of claim 169, wherein said tantalum sputtering comprises tantalum having a purity of at least 99.99% tantalum.

### Claim 175 (depends on 169)

The tantalum sputtering component of claim 169, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.995% tantalum.

### Claim 176 (depends on 169)

The tantalum sputtering component of claim 169, wherein said tantalum sputtering component comprises tantalum having a purity of at least 99.999% tantalum.

### Claim 177 (depends on 169)

The tantalum sputtering component of claim 169, wherein said tantalum sputtering component is fully recrystallized.

### Claim 178 (depends on 169)

The tantalum sputtering component of claim 169, wherein said tantalum sputtering component is at least partially recrystallized.

### Claim 179 (depends on 169)

The tantalum sputtering component of claim 169, wherein about 98% or more of said tantalum sputtering component is recrystallized.

### Claim 180 (depends on 169)

The tantalum sputtering component of claim 169, wherein about 80% or more of said tantalum sputtering component is recrystallized.

### Claim 181 (depends on 169)

The tantalum sputtering component of claim 169, wherein said average grain size is about 50 microns or less.

### Claim 182

A process of making a sputtering component from tantalum metal, comprising:
a) mechanically or chemically clean surfaces of the tantalum metal, wherein the tantalum metal has a sufficient starting cross-sectional area to permit steps b) through g);
b) flat forging the tantalum metal into at least one rolling slab, wherein the at least one rolling slab has sufficient deformation to achieve substantially uniform recrystallization after annealing in step d);
c) mechanically or chemically clean surfaces of the at least one rolling slab;
d) annealing the at least one rolling slab at a sufficient temperature and for a sufficient time to achieve at least partial recrystallization of the at least one rolling slab;
e) cold or warm rolling the at least one rolling slab in both the perpendicular and parallel directions to the axis of the starting tantalum metal to form at least one plate;
f) flattening the at least one plate; and
g) annealing the at least one plate to have an average grain size equal to or less than about 150 microns and a texture substantially void of (100) textural bands;

### Claim 183 (depends on 182)

The process of claim 182, wherein said tantalum sputtering component is a sputtering target.

### Claim 184 (depends on 182)

The process of claim 182, wherein the tantalum metal has a purity of at least 99.50%.

### Claim 185 (depends on 182)

The process of claim 182, wherein the flat forging occurs after the tantalum metal is placed in air for at least about 4 hours and from temperatures ranging from ambient to about 1200° C.

### Claim 186 (depends on 182)

The process of claim 182, wherein the cold rolling is transverse rolling at ambient temperatures and the warm rolling is at temperatures of less than about 370° C.

### Claim 187 (depends on 182)

The process of claim 182, wherein the annealing of the plate is vacuum annealing at a temperature and for a time sufficient to achieve recrystallization of the tantalum metal.

### Claim 188

A process of making a sputtering component from tantalum metal, comprising:
a) mechanically or chemically clean surfaces of the tantalum metal, wherein the tantalum metal has a sufficient starting cross-sectional area to permit steps b) through I);
b) round forging the tantalum metal into at least one rod, wherein the at least one rod has sufficient deformation to achieve substantially uniform recrystallization after annealing in step d) or step f);
c) cutting the rod into billets and mechanically or chemically clean the surfaces of the billets;
d) optionally annealing the billets to achieve at least partial recrystallization;
e) axially forging billets into preforms;
f) optionally annealing the preforms to achieve at least partial recrystallization;
g) cold rolling the performs into at least one plate; and
h) optionally mechanically or chemically clean the surfaces of the at least one plate; and
i) annealing the at least one plate to have an average grain size equal to or less than about 150 microns and a texture substantially void of (100) textural bands, wherein annealing occurs at least in step d) or f) or both.

### Claim 189 (depends on 188)

The process of claim 188, wherein said tantalum sputtering component is a sputtering target.

### Claim 190 (depends on 188)

The process of claim 188, wherein the tantalum has a purity of at least 99.50%.

### Claim 191 (depends on 188)

The process of claim 188, wherein the round forging occurs after subjecting the tantalum metal to temperatures of about 370° C. or lower.

### Claim 192 (depends on 188)

The process of claim 188, wherein prior to forging the billets, the billets are annealed.

### Claim 193 (depends on 188)

The process of claim 188, wherein prior to cold rolling of the preforms, the preforms are annealed.

### Claim 194 (depends on 188)

The process of claim 188, wherein the annealing of the preforms is vacuum annealing at a sufficient temperature and for a time to achieve recrystallization.

### Claim 195

A process of making a sputtering component comprising round forging tantalum metal into at least one rod;
annealing said at least one rod;
forging said at least one rod into at least one preform;
annealing said at least one preform;
rolling said at least one preform, and
annealing afterwards.

### Claim 196 (depends on 195)

The process of claim 195, wherein said tantalum sputtering component is a sputtering target.

### Claim 197 (depends on 195)

The process of claim 195, wherein said forging is axially.

### Claim 198 (depends on 195)

The process of claim 195, wherein said rolling is cold rolling.

### Claim 199

A process of making a sputtering component comprising;
radial forging a tantalum metal;
forging said tantalum metal after radial forging;
rolling said tantalum metal; and
annealing said tantalum metal.

### Claim 200 (depends on 199)

The process of claim 199, wherein said tantalum sputtering component is a sputtering target.

### Claim 201 (depends on 199)

The process of claim 199, wherein said sputtering component has no textural (100) bands.

### Claim 202 (depends on 199)

The process of claim 199, wherein said sputtering component has a uniform texture of mixed or primary (111) throughout the thickness of the sputtering component.

### Claim 203

A process of making a sputtering component comprising
flat forging a tantalum metal;
annealing said tantalum metal;
rolling said tantalum metal into a plate or sheet;
annealing said plate or sheet to achieve a tantalum metal having no textural (100) bands.

### Claim 204 (depends on 203)

The process of claim 203, wherein said tantalum sputtering component is a sputtering target.

### Claim 205 (depends on 203)

The process of claim 203, wherein said process further comprises flattening said tantalum metal after the last anneal and then annealing again.

### Claim 206

A process of making a sputtering component comprising a combination of cold and/or warm working of a tantalum metal and in-process annealing to obtain a uniform texture of mixed or primary (111) throughout the thickness of the tantalum metal.

### Claim 207 (depends on 206)

The process of claim 206, wherein said tantalum sputtering component is a sputtering target.

### Claim 208 (depends on 206)

The process of claim 206, wherein said cold and/or warm working comprises subjecting said tantalum metal to rolling and/or forging processes.

### Claim 209 (depends on 206)

The process of claim 206, wherein said tantalum metal has a purity of at least 99.50%.

### Claim 210 (depends on 206)

The process of claim 206, wherein said tantalum metal has a purity of at least 99.99% tantalum.

### Claim 211 (depends on 206)

The process of claim 206, wherein said tantalum metal has a purity of at least 99.995% tantalum.

### Claim 212 (depends on 206)

The process of claim 206, wherein said tantalum metal has a purity of at least 99.999% tantalum.

### Claim 213 (depends on 203)

The process of claim 203, wherein said flat forging imparts about 62% strain reduction, or an equivalent reduction in area of about 3:1.

### Claim 214 (depends on 203)

The process of claim 203, wherein the rolling imparts a strain reduction of about 87%.

### Claim 215 (depends on 203)

The process of claim 203, wherein the rolling imparts a strain reduction of about 94%.

### Claim 216 (depends on 203)

The process of claim 203, wherein the annealing of said plate or sheet is at a temperature of about 950-1050° C.

### Claim 217 (depends on 199)

The process of claim 199, wherein said radial forging imparts about 88% strain reduction, or an equivalent reduction in area of about 8.5:1.

### Claim 218 (depends on 199)

The process of claim 199, wherein said forging after radial forging imparts about 64% strain reduction.

### Claim 219 (depends on 199)

The process of claim 199, wherein said rolling imparts about 84% strain reduction.

### Claim 220 (depends on 199)

The process of claim 199, wherein the annealing after said rolling is at a temperature of 950°-1050° C.

### Claim 221 (depends on 120)

The tantalum sputtering component of claim 120 having a ratio of (111):(100) center peak intensities of greater than about −4.0.

### Claim 222 (depends on 79)

The tantalum sputtering component of claim 79, further comprising a backing plate.

### Claim 223 (depends on 86)

The tantalum sputtering component of claim 86, further comprising a backing plate.

### Claim 224 (depends on 142)

The tantalum sputtering component of claim 142, further comprising a backing plate.

### Claim 225 (depends on 149)

The tantalum sputtering component of claim 149, further comprising a backing plate.

### Claim 226 (depends on 157)

The tantalum sputtering component of claim 157, further comprising a backing plate.

### Claim 227 (depends on 172)

The tantalum sputtering component of claim 172, further comprising a backing plate.