# US 2002/0120081 A1 · Polymerization of ethylene

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2002/0120081 A1
- Document ID: US20020120081A1
- Status: Published application
- Kind: A1
- Application number: 10/134,137
- Filed: 2002-04-26
- Published: 2002-08-29
- Earliest claimed: 1999-04-01
- Assignees: E. I. Du Pont de Nemours and Company
- Inventors: Zhibin Guan
- Web page: https://patentgrep.com/patent/US20020120081A1

## CPC

- C08F 10/00: Homopolymers and copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond
- C08F 110/02: Ethene
- C08F: MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS

## Abstract

Complexes of certain transition metals with certain phosphorous-nitrogen bidentate ligands are part of all of catalyst systems for the polymerization of ethylene. Under certain polymerization conditions novel, highly branched, homopolyethylenes may be produced.

## Claims

### Claim 1

A process for the production of polyethylene, comprising the step of contacting, at a temperature of about −100° C. to about +200° C., ethylene and a Ti, Cr, V, Zr, Hf or Ni complex of a ligand of the formula
9
wherein:
T is hydrocarbylene, substituted hydrocarbylene or —CR9R10—;
R2 is hydrogen, hydrocarbyl or substituted hydrocarbyl;
R3 and R4 are each independently hydrocabyl or substituted hydrocarbyl, provided that a carbon atom bound to a nitrogen atom has at least two other carbon atoms bound to it;
R5 and R6 are each independently hydrogen, hydrocarbyl or substituted hydrocarbyl;
R7 and R8 are each independently hydrocarbyl or substituted hydrocarbyl, provided that a carbon atom bound to a phosphorous atom has at least two other carbon atoms bound to it;
R9 and R10 are each independently hydrogen, hydrocarbyl or substituted hydrocarbyl;
R11 and R12 are each independently hydrocarbyl or substituted hydrocarbyl;
R13 is hydrocarbyl or substituted hydrocarbyl;
and provided that R2 and R9 taken together may form a ring.

### Claim 2 (depends on 1)

The process as recited in claim 1, wherein one or more of the following occurs:
R3 is hydrocarbyl;
R4 is hydrogen or alkyl, hydrogen;
R and R8 are independently saturated hydrocarbyl;
R5 and R6 are independently hydrogen or methyl;
R13 is alkyl or halogen substituted aryl;
R11 and R12 are each independently hydrocarbyl or substituted hydrocarbyl;
T is —CHR14— wherein R14 is hydrogen or alkyl containing 1 to 6 carbon atoms, T is —CR9R10—, or T is o-phenylene; and
R10 is hydrogen and R2 taken together form a ring.

### Claim 3 (depends on 1)

The process as recited in claim 1, wherein one or more of the following occurs:
R3 is alkyl or alkyl or halogen substituted aryl;
R7 and R8 are independently alkyl or cycloalkyl containing 3 to 8 carbon atoms;
R5 and R6 are both hydrogen;
R13 is 2,6-disubstituted phenyl which may optionally be substituted in other positions;
R11 and R12 are each hydrocarbyl in which the carbon atom bound to the phosphorous atom is bound to at least 2 other carbon atoms;
T is —CHR14— wherein R is hydrogen or alkyl containing 1 to 6 carbon atoms, T is —CR9R10—, or T is o-phenylene; and
R10 is hydrogen and R2 taken together form a carbocyclic ring.

### Claim 4 (depends on 1)

The process as recited in claim 1 wherein said ligand is
10
wherein Me is methyl, Et is ethyl, Bu is butyl, Cy is cyclohexyl, and Ph is phenyl.

### Claim 5 (depends on 1)

The process as recited in claim 1, wherein said temperature is about 25° C. to about 100° C.

### Claim 6 (depends on 1)

The process as recited in claim 1, wherein one or more other polymerization catalysts and, optionally, one or more other monomers polymerizable by said other polymerization catalyst, is present.

### Claim 7 (depends on 1)

The process as recited in claim 1, wherein M is Ni.

### Claim 8

A process for the production of polyethylene, comprising the step of contacting, at a temperature of about −100 ° C. to about +200° C., ethylene, a compound of the formula
11
and:
(a) a first compound W. which is a neutral Lewis acid capable of abstracting X−and alkyl group or a hydride group from M to form WX−, (WR20) or WH−and which is also capable of transferring an alkyl group or a hydride to M, provided that WX−is a weakly coordinating anion; or
(b) a combination of second compound which is capable of transferring an alkyl or hydride group to M and a third compound which is a neutral Lewis acid which is capable of abstracting X−, a hydride or an alkyl group from M to form a weakly coordinating anion;
wherein:
M is Ti, Cr, V, Zr, Hf or Ni;
each X is an anion;
n is an integer so that the total number of negative charges on said anion or anions is equal to the oxidation sate of M;
T is hydrocarbylene, substituted hydrocarbylene or —CR9R10—;
R2 is hydrogen, hydrocarbyl or substituted hydrocarbyl;
R3 and R4 are each independently hydrocabyl or substituted hydrocarbyl, provided that a carbon atom bound to a nitrogen atom has at least two other carbon atoms bound to it;
R5 and R6 are each independently hydrogen, hydrocarbyl or substituted hydrocarbyl;
R7 and R8 are each independently hydrocarbyl or substituted hydrocarbyl, provided that a carbon atom bound to a phosphorous atom has at least two other carbon atoms bound to it;
R9 and R10 are each independently hydrogen, hydrocarbyl or substituted hydrocarbyl;
R11 and R12 are each independently hydrocarbyl or substituted hydrocarbyl;
R13 is hydrocarbyl or substituted hydrocarbyl; and provided that R2 and R9taken together may form a ring.

### Claim 9 (depends on 8)

The process as recited in claim 8, wherein one or more of the following occurs:
R3 is hydrocarbyl;
R4 is hydrogen or alkyl, hydrogen;
R7 and R8 are independently saturated hydrocarbyl;
R5 and R6 are independently hydrogen or methyl;
R13 is alkyl or halogen substituted aryl;
R11 and R12 are each independently hydrocarbyl or substituted hydrocarbyl;
T is —CHR14— wherein R14 is hydrogen or alkyl containing 1 to 6 carbon atoms, T is —CR9R10—, or T is o-phenylene; and
R10 is hydrogen and R2 taken together form a ring.

### Claim 10 (depends on 8)

The process as recited in claim 8, wherein one or more of the following occurs:
R3 is alkyl or alkyl or halogen substituted aryl;
R7 and R8 are independently alkyl or cycloalkyl containing 3 to 8 carbon atoms;
R5 and R6 are both hydrogen;
R13 is 2,6-disubstituted phenyl which may optionally be substituted in other positions;
R11 and R12 are each hydrocarbyl in which the carbon atom bound to the phosphorous atom is bound to at least 2 other carbon atoms;
T is —CHR14— wherein R14 is hydrogen or alkyl containing 1 to 6 carbon atoms, T is —CR9R10—, or T is o-phenylene; and
R10 is hydrogen and R2 taken together form a carbocyclic ring.

### Claim 11 (depends on 8)

The process as recited in claim 8, wherein a ligand coordinated to M is
12
wherein Me is methyl, Et is ethyl, Bu is butyl, Cy is cyclohexyl, and Ph is phenyl.

### Claim 12 (depends on 8)

The process as recited in claim 8, wherein W is an alkylaluminum compound.

### Claim 13 (depends on 8)

The process as recited in claim 8, wherein said temperature is about 25° C. to about 100° C.

### Claim 14 (depends on 12)

The process as recited in claim 12, wherein a homopolyethylene having a Mark-Houwink constant of about 1.0 or more in 1,2,4-trichlorobenzene is produced.

### Claim 15 (depends on 8)

The process as recited in claim 8, wherein one or more other polymerization catalysts and, optionally, one or more other monomers polymerizable by said other polymerization catalyst, is present.

### Claim 16 (depends on 8)

The process as recited in claim 8, wherein M is Ni.

### Claim 17

A process for the production of polyethylene, comprising the step of contacting, at a temperature of about −100 ° C. to about +200° C., ethylene and a compound of the formula
13
wherein:
M is Ti, Cr, V, Zr, Hf or Ni;
each X is an anion;
n is an integer so that the total number of negative charges on said anion or anions is equal to the oxidation sate of M;
T is hydrocarbylene, substituted hydrocarbylene or —CR9R10—;
R2 is hydrogen, hydrocarbyl or substituted hydrocarbyl;
R3 and R4 are each independently hydrocabyl or substituted hydrocarbyl, provided that a carbon atom bound to a nitrogen atom has at least two other carbon atoms bound to it;
R5 and R6 are each independently hydrogen, hydrocarbyl or substituted hydrocarbyl;
R7 and R8 are each independently hydrocarbyl or substituted hydrocarbyl, provided that a carbon atom bound to a phosphorous atom has at least two other carbon atoms bound to it;
R9 and R10 are each independently hydrogen, hydrocarbyl or substituted hydrocarbyl;
R11 and R12 are each independently hydrocarbyl or substituted hydrocarbyl;
R13 is hydrocarbyl or substituted hydrocarbyl;
Z1 is hydride or alkyl or any other anionic ligand into which ethylene can insert;
Y is a neutral ligand capable of being displaced by ethylene or a vacant coordination site;
Q is a relatively non-coordinating anion;
P is a divalent polyethylene group containing one or more ethylene molecules; and
Z2 is an end group;
and provided that R2 and R9 taken together may form a ring.

### Claim 18 (depends on 17)

The process as recited in claim 17, wherein one or more of the following occurs:
R3 is hydrocarbyl;
R4 is hydrogen or alkyl, hydrogen;
R7 and R8 are independently saturated hydrocarbyl;
R5 and R6 are independently hydrogen or methyl;
R13 is alkyl or halogen substituted aryl;
R11 and R12 are each independently hydrocarbyl or substituted hydrocarbyl;
T is —CHR14— wherein R14 is hydrogen or alkyl containing 1 to 6 carbon atoms, T is —CR9R10—, or T is o-phenylene; and
R10 is hydrogen and R taken together form a ring.

### Claim 19 (depends on 17)

The process as recited in claim 17, wherein one or more of the following occurs:
R3 is alkyl or alkyl or halogen substituted aryl;
R7 and R8 are independently alkyl or cycloalkyl containing 3 to 8 carbon atoms;
R5 and R6 are both hydrogen;
R13 is 2,6-disubstituted phenyl which may optionally be substituted in other positions;
R11 and R12 are each hydrocarbyl in which the carbon atom bound to the phosphorous atom is bound to at least 2 other carbon atoms;
T is —CHR14 wherein R14 is hydrogen or alkyl containing 1 to 6 carbon atoms, T is —CR9R10—, or T is o-phenylene; and
R10 is hydrogen and R2 taken together form a carbocyclic ring.

### Claim 20 (depends on 17)

The process as recited in claim 17, wherein said temperature is about 25° C. to about 100° C.

### Claim 21 (depends on 17)

The process as recited in claim 17, wherein one or more other polymerization catalysts and, optionally, one or more other monomers polymerizable by said other Polymerization catalyst is present.

### Claim 22 (depends on 17)

The process as recited in claim 17, wherein M is Ni.

### Claim 23

A homopolyethylene which has a Mark-Houwink constant of about 1.0 or more when measured in 1,2,4-trichlorobenzene.

### Claim 24 (depends on 23)

The homopolyethylene as recited in claim 23, wherein said constant is measured at 135° C.