# US 2002/0058209 A1 · Method of fabricating capillary discharge plasma display panel using lift-off process

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2002/0058209 A1
- Document ID: US20020058209A1
- Status: Published application
- Kind: A1
- Application number: 09/885,135
- Filed: 2001-06-21
- Published: 2002-05-16
- Earliest claimed: 2000-11-14
- Assignees: Plasmion Displays, LLC
- Inventors: Steven Kim; Geun Young Yeom; Young-Joon Lee
- Web page: https://patentgrep.com/patent/US20020058209A1

## CPC

- H01J 11/12: with main electrodes provided on both sides of the discharge space
- H01J 9/02: Manufacture of electrodes or electrode systems
- H01J 11/38: Dielectric or insulating layers
- H01J: ELECTRIC DISCHARGE TUBES OR DISCHARGE LAMPS (spark-gaps H01T; electric arc lamps H05B31/00; particle accelerators H05H)

## Abstract

A method for fabricating a PDP is disclosed. The method for fabricating a PDP comprising the steps of preparing first and second panels for connecting with each other, forming at least one electrode on the first panel, forming a dielectric layer of PbO on the first panel, sequentially forming Cr and Ni on the PbO layer as a mask material of the PbO layer, performing photolithography and lift-off processes on the Ni/Cr layers to form a mask pattern of Ni/Cr, and etching the PbO layer using the mask pattern of Ni/Cr to form at least one capillary tube within the PbO layer to expose the electrode.

## Claims

### Claim 1

A method for fabricating a plasma display panel having first and second panels, the method comprising the steps of:
forming at least one electrode on the first panel;
forming a dielectric layer of PbO on the first panel;
sequentially forming Cr and Ni layers on the PbO layer as a mask of the PbO layer;
performing photolithography and lift-off processes on the Cr and Ni layers to form a mask pattern of the Cr and Ni; and
etching the PbO layer using the mask pattern of Ni/Cr to form at least one capillary tube within the PbO layer to expose the electrode.

### Claim 2 (depends on 1)

The method of claim 1, wherein the panels are glass substrates.

### Claim 3 (depends on 1)

The method of claim 1, wherein the Cr and Ni are deposited by electron-beam evaporation method.

### Claim 4 (depends on 1)

The method of claim 1, wherein the Ni layer has a thickness of 1.5 m and the Cr layer has a thickness of 4000 when the PbO layer has a thickness of 15 m.

### Claim 5 (depends on 1)

The method of claim 1, wherein the step of forming the mask pattern of Ni/Cr includes the steps of:
depositing a negative photoresist on the Ni/Cr layers and performing the photolithography process to form a picture inverted photoresist pattern of the capillary tube; and
performing the lift-off process on the Ni/Cr layers using the photoresist pattern to form the mask pattern of Ni/Cr.

### Claim 6 (depends on 5)

The method of claim 5, wherein the negative photoresist is AZ 5214E picture inverted photoresist.

### Claim 7 (depends on 1)

The method of claim 1, wherein the PbO layer is etched by dry etching process, and the etching process has conditions such as etch gas of CF4+20% Ar, panel temperature of 70 C., inductive power of 900 W, bias voltage of −200 V, and process pressure of 7 mTorr.

### Claim 8 (depends on 1)

The method of claim 1, wherein the Ni layer has a thickness of 1.1 m and the Cr layer has a thickness of 1000 when the PbO layer has a thickness of 10 m.

### Claim 9 (depends on 1)

The method of claim 1, wherein the lift-off process is performed using acetonic ultrasonic cleaning.

### Claim 10

A method for fabricating a PDP comprising the steps of:
preparing a first and second panels;
depositing a dielectric layer on a first panel;
depositing at least one film on the dielectric layer;
forming a photoresist pattern on the film;
performing a lift-off process of the film; and
forming at least one channel within the dielectric layer.

### Claim 11 (depends on 10)

The method of claim 10, wherein the panels are glass panels.

### Claim 12 (depends on 10)

The method of claim 10, wherein at least one electrode is formed on the first panel.

### Claim 13 (depends on 10)

The method of claim 10, wherein the dielectric layer is a PbO layer.

### Claim 14 (depends on 10)

The method of claim 10, wherein the film is a Cr/Ni film.

### Claim 15 (depends on 14)

The method of claim 14, wherein the Cr film is deposited by electron-beam evaporation.

### Claim 16 (depends on 14)

The method of claim 14, wherein the Ni film is deposited by sputtering.

### Claim 17 (depends on 10)

The method of claim 10, wherein the photoresist pattern is an AZ 5214E picture inverted pattern.

### Claim 18 (depends on 10)

The method of claim 10, wherein the lift-off process is performed by acetonic ultrasonic cleaning.

### Claim 19 (depends on 10)

The method of claim 10, wherein the at least one channel is formed by etching the layer using the pattern formed by a lift-off process as a mask.