# US 2001/0034121 A1 · High selectivity Si-rich SiON etch-stop layer

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2001/0034121 A1
- Document ID: US20010034121A1
- Status: Published application
- Kind: A1
- Application number: 09/838,627
- Filed: 2001-04-20
- Published: 2001-10-25
- Earliest claimed: 1999-02-05
- Assignees: Taiwan Semiconductor Manufacturing Company, Ltd.
- Inventors: Chu Yun Fu; Chia Shiung Tsai; Syun-Ming Jang
- Web page: https://patentgrep.com/patent/US20010034121A1

## CPC

- H10P 14/6927: {the material being a silicon oxynitride, e.g. SiON or SiON:H}
- H10P 14/6334: {using decomposition or reaction of gaseous or vapour phase compounds, i.e. chemical vapour deposition (deposition by physical ablation of a target H10P14/6329)}
- H10P 14/6682: {the compound being a silane, e.g. disilane, methylsilane or chlorosilane}
- H10P 14/69215: {the material being a silicon oxide, e.g. SiO2}
- H10P 50/283: {by chemical means}
- H10P 76/2043: {using an anti-reflective coating}
- H10P 76/405: {characterised by their composition, e.g. multilayer masks}
- H10P 76/4085: {characterised by the processes involved to create the masks}
- H10W 20/071: {of dielectric parts thereof}
- H10W 20/074: {of dielectric parts comprising thin functional dielectric layers, e.g. dielectric etch-stop, barrier, capping or liner layers}
- H10W 20/086: {involving buried masks}
- H10W 20/088: {involving partial etching of via holes}
- H10P: GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
- H10W: GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10

## Abstract

The present invention provides an anti-reflective Si-Rich Silicon oxynitride (SiON) etch barrier layer and two compatible oxide etch processes. The Si-Rich Silicon oxynitride (SiON) etch barrier layer can be used as a hard mask in a dual damascene structure and as a hard mask for over a polysilicon gate. The invention has the following key elements: 1) Si rich Silicon oxynitride (SiON) ARC layer, 2) Special Silicon oxide Etch process that has a high selectivity of Si- Rich SiON to silicon oxide or SiN; 3) Special Si Rich SiON spacer process for a self aligned contact (SAC). A dual damascene structure is formed by depositing a first dielectric layer. A novel anti-reflective Si-Rich Silicon oxynitride (SiON) etch barrier layer is deposited on top of the first dielectric layer. A first opening is etched in the first insulating layer. A second dielectric layer is deposited on the anti-reflective Si-Rich Silicon oxynitride (SiON) etch barrier layer. A second dual damascene opening is etched into the dielectric layers. The anti-reflective Si-Rich Silicon oxynitride (SiON) etch barrier layer can also serve as an ARC layer during these operations to reduce the amount of reflectance from conductive region to reduce distortion of the photoresist pattern.

## Claims

### Claim 1

A method for forming a dual damascene interconnect using an Anti-Reflective Coating (ACR) etch stop layer composed of Si Rich SiON, the method comprising the steps of
a) forming a conductive line over said substrate;
b) forming a first insulating layer overlying the conductive line;
c) forming an ARC etch stop layer composed of Si Rich SiON overlying the first insulating layer; said ARC etch stop layer has a RI between about 2.6 and 2.8 measured at 633 nm;
d) forming a first photoresist layer overlying said first insulating layer;
e) exposing said first photoresist layer to light to molecularly alter a portion of the first photoresist layer wherein the ARC etch stop layer attenuates light reflected from the conductive region so that the light reflected from the conductive region has a reduced effect on the portion of the first photoresist layer which is molecularly altered;
f) developing said first photoresist layer to form a first photoresist opening;
g) etching said first dielectric layer thorough said first photoresist opening forming a first opening;
h) removing said first photoresist layer;
i) forming a second insulating layer over said ARC etch stop layer and said first dielectric layer;
j) forming a second photoresist layer on said second insulating layer;
k) exposing said second photoresist layer to light to molecularly alter a portion of the second photoresist layer wherein said ARC etch stop layer attenuates light reflected from said conductive region so that the light reflected from said conductive region has a reduced effect on the portion of the second photoresist layer which is molecularly altered;
l) developing said second photoresist layer to form a second photoresist opening;
m) etching said second insulating layer thorough said second photoresist opening forming a second opening and wherein said ARC etch stop layer is used as an etch stop layer; and etching said first insulating layer extending said first opening to expose said conductive line; said first and said second openings comprise a dual damascene opening;
n) remove said second photoresist layer;
o) depositing a metal layer so that the metal layer fills said first and second opening; and
p) planarizing said metal layer so that the metal layer forms an electrical interconnect which is electrically coupled to the conductive region.

### Claim 2 (depends on 1)

The method of claim 1 wherein said ARC etch stop layer is composed of Si-rich SiON and is formed by the following process: a Pressure (Torr) between about 4 and 6 Torr, a power between 100 and 150 Watt; an electrode spacing between 450 and 550 mils, a SiH4 flow between 70 and 90 SCCM, a N2O flow between 30 and 50 SCCM and a He flow between 1900 and 2500 SCCM, at a temperature between 300 and 400° C.

### Claim 3 (depends on 1)

The method of claim 1 wherein said ARC etch stop layer is composed of Si-rich SION having a Si molar percentage between about 58% and 62% and is formed by the following process: a Pressure (Torr) between about 4 and 6 Torr, a power between 100 and 150 Watt; an electrode spacing between 450 and 550 mils, a SiH4 flow between 70 and 90 SCCM, a N2O flow between 30 and 50 SCCM and a He flow between 1900 and 2500 SCCM, at a temperature between 300 and 400° C., and said ARC etch stop layer having a refractive index (RI) between 2.65 and 2.75 measure at 633 nm.

### Claim 4 (depends on 1)

The method of claim 1 wherein said conductive line is comprised of a material selected from the group consisting of an Al Alloy, a polysilicon, and a polycide.

### Claim 5 (depends on 1)

The method of claim 1 wherein said light has a wavelength within the range of 364 nm to 366 nm.

### Claim 6 (depends on 1)

The method of claim 1 wherein said light has a wavelength within the range of 247 nm to 249 nm.

### Claim 7 (depends on 1)

The method of claim 1 wherein the etching of said second insulating layer is preformed at the following: a Pressure (torr) between 100 and 250 mtorr, a Power (W) between 900 and 1200 W; a CHF3 flow between 60 and 95 sccm; a CF4 flow (Sccm) between 5 and 30 sccm, a Ar flow (Sccm) between 100 and 200 sccm Ar, a Magnetic Field between 0 and 50 G; an etch selectivity between Si-rich SiON: oxide between 1:4.2 and 1:5.7; and an Etch selectivity of SiON: oxide between 1:1.5 and 1:4; an etch selectivity PE nitride: oxide between 1:1.5 and 1:3; and said second insulating layer is composed of silicon oxide.

### Claim 8 (depends on 1)

The method of claim 1 wherein the etching of said second insulating layer 44 is preformed at the following: a pressure between 1 and 15 mtorr; a power between 900 and 1500 W, a bias Power (watts) 1000 and 1800 W; a C2F6 flow (sccm) between 7 and 9 sccm; and C4F8 flow between 10 and 20 sccm; an Ar flow between 100 and 200 sccm; and Etch selectivity between Si-rich SiON: oxide at about 1:7 and 1:15; an etch selectivity of SiON: oxide between 1:1.5 and 1:4; and said second insulating layer is composed of silicon oxide.

### Claim 9

A method for forming a dual damascene interconnect using an Anti-Reflective Coating etch stop layer composed of Si Rich SiON, the method comprising the steps of:
a) forming a conductive line over said substrate; said conductive line is comprised an Al Alloy;
b) forming a first insulating layer overlying the conductive line;
c) forming an ARC etch stop layer composed of Si Rich SiON overlying the first insulating layer;
(c-1) said ARC etch stop layer is composed of Si-rich SiON having a Si molar percentage between about 58% and 62% formed by the following process: a Pressure (Torr) between about 4 and 6 Torr, a power between 100 and 150 Watt; an electrode spacing between 450 and 550 mils, a SiH4 flow between 70 and 90 SCCM, a N2O flow between 30 and 50 SCCM and a He flow between 1900 and 2500 SCCM, at a temperature between 300 and 400° C., and said ARC etch stop layer having a refractive index (RI) between 2.65 and 2.75 measure at 633 nm;
d) forming a first photoresist layer overlying said first insulating layer;
e) exposing said first photoresist layer to light to molecularly alter a portion of the first photoresist layer wherein the ARC etch stop layer attenuates light reflected from the conductive region so that the light reflected from the conductive region has a reduced effect on the portion of the first photoresist layer which is molecularly altered; said light has a wavelength within the range of 364 nm to 366 nm;
f) developing said first photoresist layer to form a first photoresist opening;
g) etching said first dielectric layer thorough said first photoresist opening forming a first opening;
h) removing said first photoresist layer;
i) forming a second insulating layer over said ARC etch stop layer and said first dielectric layer;
j) forming a second photoresist layer on said second insulating layer;
k) exposing said second photoresist layer to light to molecularly alter a portion of the second photoresist layer wherein said ARC etch stop layer attenuates light reflected from said conductive region so that the light reflected from said conductive region has a reduced effect on the portion of the second photoresist layer which is molecularly altered;
l) developing said second photoresist layer to form a second photoresist opening;
m) etching said second insulating layer thorough said second photoresist opening forming a second opening and wherein said ARC etch stop layer is used as an etch stop layer; and etching said first insulating layer extending said first opening to expose said conductive line; said first and said second openings comprise a dual damascene opening;
n) removing said second photoresist layer;
o) depositing a metal layer so that the metal layer fills said first and second opening; and
p) planarizing said metal layer so that the metal layer forms an electrical interconnect which is electrically coupled to the conductive region.

### Claim 10 (depends on 9)

The method of claim 9 wherein the etching of said second insulating layer is preformed at the following: a Pressure (torr) between 100 and 250 mtorr, a Power (W) between 900 and 1200 W; a CHF3 flow between 60 and 95 sccm; a CF4 flow (Sccm) between 5 and 30 sccm, a Ar flow (Sccm) between 100 and 200 sccm Ar, a Magnetic Field between 0 and 50 G; an etch selectivity between Si-rich SiON: oxide between 1:4.2 and 1:5.7; and an Etch selectivity SiON: oxide between 1:1.5 and 1:4; an etch selectivity PE nitride: oxide between 1:1.5 and 1:3; and said second insulating layer is composed of silicon oxide.

### Claim 11 (depends on 9)

The method of claim 9 wherein the etching of said second insulating layer is preformed at the following: a pressure between 1 and 15 mtorr; a power between 900 and 1500 W, a bias Power (watts) 1000 and 1800 W; a C2F6 flow (sccm) between 7 and 9 sccm; and C4F8 flow between 10 and 20 sccm; an Ar flow between 100 and 200 sccm; and Etch selectivity between Si-rich SiON: oxide at about 1:7 and 1:15; an etch selectivity: SiON: oxide between 1:1.5 and 1:4; and said second insulating layer is composed of silicon oxide.

### Claim 12

A method of fabricating a self-aligned contact to a substrate using a Si Rich Silicon oxynitride etch barrier layer and a Si Rich spacer; comprising the steps of:
a) forming a polysilicon layer over a substrate;
b) forming a hard mask layer on said polysilicon layer; said hard mask layer comprised of a bottom hard mask on a Silicon oxynitride hard mask;
(b-1) said Silicon oxynitride hard mask is composed of Si-rich SiON having a Si molar percentage between about 58% and 62%, formed by the following process: a Pressure (Torr) between about 4 and 6 Torr, a power between 100 and 150 Watt; an electrode spacing between 450 and 550 mils, a SiH4 flow between 70 and 90 SCCM, a N2O flow between 30 and 50 SCCM and a He flow between 1900 and 2500 SCCM, at a temperature between 300 and 400° C., and said silicon oxynitride layer having a refractive index (RI) between 2.65 and 2.75 measure at 633 nm;
c) patterning said hard mask layer to form a hard mask that defines a gate electrode; said gate electrode having sidewalls;
d) patterning said polysilicon layer, using said hard mask as an etch mask, to form said gate electrode;
e) forming first spacers on said sidewalls of said gate electrode; said first spacers are composed of silicon nitride or oxide formed using a LP TEOS process;
f) forming second spacers over said first spacers;
(f-1) said second spacers are composed of Si-rich SiON having a Si molar percentage between about 58% and 62% formed by the following process: a Pressure (Torr) between about 4 and 6 Torr, a power between 100 and 150 Watt; an electrode spacing between 450 and 550 mils, a SiH4 flow between 70 and 90 SCCM, a N2O flow between 30 and 50 SCCM and a He flow between 1900 and 2500 SCCM, at a temperature between 300 and 400° C., and said second spacers having a refractive index (RI) between 2.65 and 2.75 measure at 633 nm;
g) forming a bottom etch stop layer composed of silicon nitride over said second spacers, and elsewhere over said substrate;
h) forming a first insulating layer (IMD) over said bottom etch stop layer;
i) forming an ARC etch stop layer over said first insulating layer;
(i-1) said ARC etch stop layer is composed of Si-rich Silicon oxynitride having a Si molar percentage between about 58% and 62% and a Refractive index between 2.68 and 2.72 at a wavelength of about 633 nm;
j) forming a first photoresist layer having a first opening by exposing said photoresist layer to a first light and developing said first photoresist layer;
k) patterning said ARC etch stop layer using said first photoresist layer to form a first opening through said first insulating layer exposing said substrate.

### Claim 13 (depends on 12)

The method of claim 12 wherein said ARC etch stop layer is composed of Si-rich SiON formed by the following process: a Pressure (Torr) between about 4 and 6 Torr, a power between 100 and 150 Watt; an electrode spacing between 450 and 550 mils, a SiH4 flow between 70 and 90 SCCM, a N2O flow between 30 and 50 SCCM and a He flow between 1900 and 2500 SCCM, at a temperature between 300 and 400° C., and said ARC etch stop layer having a refractive index (RI) between 2.65 and 2.75 nm measured at a wavelength of about 633 nm.

### Claim 14 (depends on 12)

The method of claim 12 wherein the etch of the said first insulating layer, is preformed at the following: a Pressure (torr) between 100 and 250 mtorr, a Power (W) between 900 and 1200 W; a CHF3 flow between 60 and 95 sccm; a CF4 flow (Sccm) between 5 and 30 sccm, a Ar flow (Sccm) between 100 and 200 sccm Ar, a Magnetic Field between 0 and 50 G; an etch selectivity between Si-rich SiON: oxide between 1:4.2 and 1:5.7; and an Etch selectivity SiON: oxide between 1:2.7 and 1:4.2; an etch selectivity PE nitride: oxide between 1:1.5 and 1:3.

### Claim 15

A method of fabricating a self-aligned contact to a substrate using a Si Rich Silicon oxynitride etch barrier layer and a Si Rich spacer; comprising the steps of:
a) forming a polysilicon layer over a substrate;
b) forming a hard mask layer on said polysilicon layer; said hard mask layer comprised of a bottom hard mask on a Silicon oxynitride hard mask;
(b-1) said silicon oxynitride hard mask is composed of Si-rich SiON having a Si molar percentage between about 58% and 62% formed by the following process: a Pressure (Torr) between about 4 and 6 Torr, a power between 100 and 150 Watt; an electrode spacing between 450 and 550 mils, a SiH4 flow between 70 and 90 SCCM, a N2O flow between 30 and 50 SCCM and a He flow between 1900 and 2500 SCCM, at a temperature between 300 and 400° C., and said silicon oxynitride hard mask having a refractive index (RI) between 2.65 and 2.75 measure at 633 nm;
c) patterning said hard mask layer to form a hard mask that defines a gate electrode; said gate electrode having sidewalls;
d) patterning said polysilicon layer, using said hard mask as an etch mask, to form said gate electrode;
e) forming first spacers on said sidewalls of said gate electrode; said first spacers composed of silicon nitride or oxide formed using a LP TEOS process;
f) forming second spacers over said first spacers;
(f-1) said second spacers are composed of Si-rich SiON having a Si molar percentage between about 58% and 62% formed by the following process: a Pressure (Torr) between about 4 and 6 Torr, a power between 100 and 150 Watt; an electrode spacing between 450 and 550 mils, a SiH4 flow between 70 and 90 SCCM, a N2O flow between 30 and 50 SCCM and a He flow between 1900 and 2500 SCCM, at a temperature between 300 and 400° C., and said second spacers having a refractive index (RI) between 2.65 and 2.75 measure at 633 nm;
g) forming a bottom etch stop layer composed of silicon nitride over said second spacers, and elsewhere over said substrate;
h) forming a first insulating layer (IMD) over said bottom etch stop layer;
i) forming an ARC etch stop layer over said first insulating layer;
(i-1) said ARC etch stop layer is composed of Si-rich Silicon oxynitride having a Si molar percentage between about 58% and 62% and a Refractive index between 2.68 and 2.72 at a wavelength of about 633 mn; said ARC etch stop layer is composed of Si-rich SiON formed by the following process: a Pressure (Torr) between about 4 and 6 Torr, a power between 100 and 150 Watt; an electrode spacing between 450 and 550 mils, a SiH4 flow between 70 and 90 SCCM, a N2O flow between 30 and 50 SCCM and a He flow between 1900 and 2500 SCCM, at a temperature between 300 and 400° C., and said ARC etch stop layer having a refractive index (RI) between 2.65 and 2.75 nm measured at a wavelength of about 633 nm;
j) forming a first photoresist layer having a first opening by exposing said photoresist layer to a first light and developing said first photoresist layer;
k) patterning said ARC etch stop layer using said first photoresist layer to form a first etch stop opening through said ARC etch stop layer; and
l) etching said first insulating layer to form a contact opening exposing said substrate, the etching of said first insulating layer, is preformed at the following: a Pressure (torr) between 100 and 250 mtorr, a Power (W) between 900 and 1200 W; a CHF3 flow between 60 and 95 sccm; a CF4 flow (Sccm) between 5 and 30 sccm, a Ar flow (Sccm) between 100 and 200 sccm Ar, a Magnetic Field between 0 and 50 G; an etch selectivity between Si-rich SiON oxide between 1:4.2 and 1:5.7; and an etch selectivity SiON: oxide between 1:2.7 and 1:4.2; an etch selectivity PE SiN: oxide between 1:1.5 and 1:3.