# US 2001/0034096 A1 · Methods to form electronic devices

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2001/0034096 A1
- Document ID: US20010034096A1
- Status: Published application
- Kind: A1
- Application number: 09/539,641
- Filed: 2000-03-30
- Published: 2001-10-25
- Earliest claimed: 1998-08-24
- Assignees: Micron Technology, Inc.
- Inventors: Randhir P. S. Thakur
- Web page: https://patentgrep.com/patent/US20010034096A1

## CPC

- H10P 14/69433: {the material being a silicon nitride not containing oxygen, e.g. SixNy or SixByNz}
- H10D 1/68: Capacitors having no potential barriers
- H10P 14/6304: {Formation by oxidation, e.g. oxidation of the substrate}
- H10P 14/6322: {Formation by thermal treatments (formation by plasma treatment H10P14/6319)}
- H10B 12/033: {the capacitor extending over the transistor}
- H10P 14/6308: {of Group IV semiconductors}
- H10P 14/6309: {of silicon in uncombined form, i.e. pure silicon}
- H10P 14/6336: {in the presence of a plasma [PECVD]}
- H10P 14/662: {Laminate layers, e.g. stacks of alternating high-k metal oxides (adhesion layers or buffer layers H10P14/6508, H10P14/6548)}
- H10P 14/69215: {the material being a silicon oxide, e.g. SiO2}
- Y10S 438/954: Making oxide-nitride-oxide device
- H10P: GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
- H10D: INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
- H10B: ELECTRONIC MEMORY DEVICES
- Y10S: TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS

## Abstract

A first electrode and a doped oxide layer laterally proximate thereof are provided over a substrate. A silicon nitride layer is formed over both the doped oxide layer and the first electrode to a thickness of no greater than 80 Angstroms over at least the first electrode by low pressure chemical vapor deposition at a pressure of at least 1 Torr, a temperature of less than 700° C. and using feed gases comprising a silicon hydride and ammonia. The substrate with silicon nitride layer is exposed to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the silicon nitride layer, with the thickness of silicon nitride over the doped oxide layer being sufficient to shield oxidizable substrate material beneath the doped oxide layer from oxidizing during the exposing. A second electrode is formed over the silicon dioxide layer and the first electrode. In another implementation, a layer comprising undoped oxide is formed over a doped oxide layer. A first electrode is formed proximate the undoped oxide layer and the undoped oxide layer. With the undoped oxide layer being outwardly exposed, a silicon nitride layer is formed on the undoped oxide layer and over the first electrode by low pressure chemical vapor deposition to a thickness of no greater than 80 Angstroms. Also disclosed are methods of forming transistor gate constructions and methods of forming electronic device constructions incorporating high K dielectric layer constructions.

## Claims

### Claim 1

A method of forming an electronic device comprising:
providing a first electrode and a doped oxide layer laterally proximate thereof over a substrate;
forming a silicon nitride layer over both the doped oxide layer and the first electrode to a thickness of no greater than 80 Angstroms over at least the first electrode by low pressure chemical vapor deposition at a pressure of at least 1 Torr, a temperature of less than 700° C. and using feed gases comprising a silicon hydride and ammonia;
exposing the substrate with silicon nitride layer to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the silicon nitride layer, with the thickness of silicon nitride over the doped oxide layer being sufficient to shield oxidizable substrate material beneath the doped oxide layer from oxidizing during the exposing; and
forming a second electrode over the silicon dioxide layer and the first electrode.

### Claim 2 (depends on 1)

The method of claim 1 after forming said silicon nitride layer, forming a secondary silicon nitride layer on said silicon nitride layer by low pressure chemical vapor deposition at a pressure of less than 1 Torr, a temperature of at least 700° C. and using feed gases comprising a silicon hydride and ammonia; the secondary layer of silicon nitride being formed to provide a combined thickness of said silicon nitride layer and the secondary silicon nitride layer of no greater than 80 Angstroms over the first electrode.

### Claim 3 (depends on 1)

The method of claim 1 wherein the silicon nitride layer is formed to a thickness of less than 80 Angstroms over the doped oxide layer.

### Claim 4 (depends on 1)

The method of claim 1 wherein the silicon nitride layer is formed on the doped oxide layer.

### Claim 5 (depends on 1)

The method of claim 1 wherein the first electrode is outwardly exposed during the forming of the silicon nitride layer thereover.

### Claim 6 (depends on 1)

The method of claim 1 wherein the first electrode is not outwardly exposed during the forming of the silicon nitride layer thereover.

### Claim 7 (depends on 1)

The method of claim 1 wherein the first electrode is covered with an oxide layer during the forming of the silicon nitride layer thereover.

### Claim 8 (depends on 1)

The method of claim 1 wherein the doped oxide layer comprises BPSG.

### Claim 9 (depends on 1)

The method of claim 1 wherein the pressure during the forming of the silicon nitride is less than or equal to 2.5 Torr.

### Claim 10 (depends on 1)

The method of claim 1 wherein the temperature during the forming of the silicon nitride is less than or equal to 650° C.

### Claim 11 (depends on 1)

The method of claim 1 wherein the pressure during the forming of the silicon nitride is less than or equal to 2.5 Torr, and the temperature during the forming of the silicon nitride is less than or equal to 650° C.

### Claim 12 (depends on 1)

The method of claim 1 wherein the silicon nitride is formed by plasma deposition.

### Claim 13 (depends on 1)

The method of claim 1 wherein the silicon nitride is formed to a thickness no greater than 60 Angstroms.

### Claim 14

A method of forming an electronic device comprising:
providing a first electrode and a doped oxide layer laterally proximate thereof over a substrate;
forming a first silicon nitride layer over both the doped oxide layer and the first electrode to a thickness of no greater than 70 Angstroms over at least the first electrode by low pressure chemical vapor deposition using a first set of reactor conditions using feed gases comprising a silicon hydride and ammonia;
after using the first set of conditions, forming a second silicon nitride layer on the first silicon nitride layer to a thickness of no greater than 70 Angstroms over at least the first electrode by low pressure chemical vapor deposition using a second set of reactor conditions using feed gases comprising a silicon hydride and ammonia, the second layer being formed to provide a combined thickness of the first and second nitride layers of no greater than 80 Angstroms over the first electrode;
exposing the substrate with the first and second silicon nitride layers to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the second silicon nitride layer, with the thickness of silicon nitride over the doped oxide layer being sufficient to shield oxidizable substrate material beneath the doped oxide layer from oxidizing during the exposing; and
forming a second electrode over the silicon dioxide layer and the first electrode.

### Claim 15 (depends on 14)

The method of claim 14 wherein the second silicon nitride layer is formed to provide a combined thickness of the first and second nitride layers of no greater than 60 Angstroms over the first electrode.

### Claim 16 (depends on 14)

The method of claim 14 wherein the first silicon nitride layer is formed on the doped oxide layer.

### Claim 17 (depends on 14)

The method of claim 14 wherein the first electrode is outwardly exposed during the forming of the silicon nitride layer thereover.

### Claim 18 (depends on 14)

The method of claim 14 wherein the first electrode is not outwardly exposed during the forming of the silicon nitride layer thereover.

### Claim 19 (depends on 14)

The method of claim 14 wherein the first electrode is covered with an oxide layer during the forming of the silicon nitride layer thereover.

### Claim 20

A method of forming an electronic device comprising:
providing a first electrode and a doped oxide layer laterally proximate thereof over a substrate;
first exposing the doped oxide layer to rapid thermal nitridation conditions effective to grow a seed nitride layer over at least the doped oxide layer to a thickness of at least about 8 Angstroms;
forming a silicon nitride layer over both the seed nitride layer and the first electrode by low pressure chemical vapor deposition at a pressure of less than 1 Torr, a temperature of at least 700° C. and using feed gases comprising a silicon hydride and ammonia, a combined thickness of the silicon nitride layer and any seed nitride layer formed over the first electrode being no greater than 80 Angstroms;
second exposing the substrate with the silicon nitride layer to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the silicon nitride layer, with the thickness of the silicon nitride layer and the seed layer over the doped oxide layer being sufficient to shield oxidizable substrate material beneath the doped oxide layer from oxidizing during the second exposing; and
forming a second electrode over the silicon dioxide layer and the first electrode.

### Claim 21 (depends on 20)

The method of claim 20 wherein the seed layer is grown to a thickness of no greater than 20 Angstroms.

### Claim 22 (depends on 20)

The method of claim 20 wherein the combined thickness of the silicon nitride layer and any seed nitride layer formed over the first electrode is no greater than 60 Angstroms.

### Claim 23 (depends on 20)

The method of claim 20 wherein the conditions are effective to grow the seed layer over both the electrode and doped oxide layer to respective thicknesses of at least about 8 Angstroms.

### Claim 24 (depends on 20)

The method of claim 20 wherein the silicon nitride layer is formed on the doped oxide layer.

### Claim 25 (depends on 20)

The method of claim 20 wherein the first electrode is outwardly exposed during the first exposing, with the seed layer forming on the first electrode.

### Claim 26 (depends on 20)

The method of claim 20 wherein the first electrode is not outwardly exposed during the first exposing.

### Claim 27 (depends on 20)

The method of claim 20 wherein the first electrode is covered with an oxide layer during the first exposing.

### Claim 28

A method of forming an electronic device comprising:
providing a first electrode and a doped oxide layer laterally proximate thereof over a substrate;
first exposing the doped oxide layer to rapid thermal nitridation conditions effective to grow a seed nitride layer over at least the doped oxide layer to a thickness of at least about 8 Angstroms;
forming a silicon nitride layer over both the seed nitride layer and the first electrode by low pressure chemical vapor deposition at a pressure of at least 1 Torr, a temperature of less than 700° C. and using feed gases comprising a silicon hydride and ammonia, a combined thickness of the silicon nitride layer and any seed nitride layer formed over the first electrode being no greater than 80 Angstroms;
second exposing the substrate with the silicon nitride layer to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the silicon nitride layer, with the thickness of the silicon nitride layer and the seed layer over the doped oxide layer being sufficient to shield oxidizable substrate material beneath the doped oxide layer from oxidizing during the second exposing; and
forming a second electrode over the silicon dioxide layer and the first electrode.

### Claim 29 (depends on 28)

The method of claim 28 wherein the seed layer is grown to a thickness of no greater than 20 Angstroms.

### Claim 30 (depends on 28)

The method of claim 28 wherein the combined thickness of the silicon nitride layer and any seed nitride layer formed over the first electrode is no greater than 60 Angstroms.

### Claim 31 (depends on 28)

The method of claim 28 wherein the conditions are effective to grow the seed layer over both the electrode and doped oxide layer to respective thicknesses of at least about 8 Angstroms.

### Claim 32

A method of forming an electronic device comprising:
providing a first electrode and a doped oxide layer laterally proximate thereof over a substrate;
forming a silicon nitride layer at least over the first electrode to a thickness of no greater than 80 Angstroms by low pressure chemical vapor deposition using feed gases comprising a silicon hydride and ammonia;
after forming the silicon nitride layer, exposing the substrate to a nitrogen containing atmosphere which is substantially void of silicon hydride at a temperature of at least about 850° C.;
after exposing the substrate to the nitrogen containing atmosphere, exposing the substrate to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the silicon nitride layer, with the exposing conditions and exposing time being effective to prevent oxidizable substrate material beneath the doped oxide layer from oxidizing during the exposing; and
forming a second electrode over the silicon dioxide layer and the first electrode.

### Claim 33 (depends on 32)

The method of claim 32 wherein the forming of said silicon nitride layer comprises a pressure of at least 1 Torr and a temperature of less than 700° C.

### Claim 34 (depends on 32)

The method of claim 32 wherein prior to forming said silicon nitride layer, initially exposing the doped oxide layer to rapid thermal nitridation conditions effective to grow a seed nitride layer over at least the doped oxide layer to a thickness of at least about 8 Angstroms.

### Claim 35 (depends on 34)

The method of claim 34 wherein the forming of said silicon nitride layer comprises a pressure of at least 1 Torr and a temperature of less than 700° C.

### Claim 36 (depends on 34)

The method of claim 34 wherein the forming of said silicon nitride layer comprises a pressure of less than 1 Torr and a temperature of at least 700° C.

### Claim 37 (depends on 32)

The method of claim 32 wherein the nitrogen containing atmosphere comprises ammonia.

### Claim 38 (depends on 32)

The method of claim 32 wherein the nitrogen containing atmosphere comprises an oxynitride compound.

### Claim 39

A method of forming an electronic device comprising:
forming a layer comprising undoped oxide over a layer of doped oxide;
forming a first electrode proximate the undoped oxide layer and the doped oxide layer;
with the undoped oxide layer being outwardly exposed, forming a silicon nitride layer on the undoped oxide layer and over the first electrode by low pressure chemical vapor deposition to a thickness of no greater than 80 Angstroms;
exposing the substrate with silicon nitride layer to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the silicon nitride layer, with the thickness of silicon nitride on the undoped oxide layer being sufficient to shield oxidizable substrate material beneath the doped oxide layer from oxidizing during the exposing; and
forming a second electrode over the silicon dioxide layer and the first electrode.

### Claim 40 (depends on 39)

The method of claim 39 wherein the undoped oxide layer is formed in situ with a chemical vapor depositing of the doped oxide layer by substantially ceasing flow of doping gas at the conclusion of the doped oxide layer deposition.

### Claim 41 (depends on 39)

The method of claim 39 wherein the silicon nitride is formed to a thickness no greater than 60 Angstroms.

### Claim 42 (depends on 39)

The method of claim 39 further comprising removing a portion of the undoped oxide layer prior to forming the first electrode.

### Claim 43 (depends on 39)

The method of claim 39 further comprising removing a portion of the undoped oxide layer by chemical-mechanical polishing prior to forming the first electrode.

### Claim 44 (depends on 39)

The method of claim 39 wherein the undoped oxide layer is formed by chemical vapor deposition and to a first thickness, and further comprising removing at least 50% of the first thickness of the undoped oxide layer prior to forming the first electrode.

### Claim 45 (depends on 39)

The method of claim 39 wherein the undoped oxide layer is formed by chemical vapor deposition and to a first thickness, and further comprising removing at least 50% of the first thickness of the undoped oxide layer by chemical-mechanical polishing prior to forming the first electrode.

### Claim 46 (depends on 39)

The method of claim 39 wherein the silicon nitride is formed to a thickness no greater than 60 Angstroms.

### Claim 47 (depends on 39)

The method of claim 39 wherein the first electrode is outwardly exposed during the forming of the silicon nitride layer thereover.

### Claim 48 (depends on 39)

The method of claim 39 wherein the first electrode is not outwardly exposed during the forming of the silicon nitride layer thereover.

### Claim 49 (depends on 39)

The method of claim 39 wherein the first electrode is covered with an oxide layer during the forming of the silicon nitride layer thereover.

### Claim 50

A method of forming a transistor gate construction comprising:
providing a semiconductive region of a substrate to be gated;
providing a conductive transistor gate proximate the region to be gated;
providing a gate dielectric layer intermediate the region to be gated and the transistor gate, the gate dielectric layer being at least partially provided by low pressure chemical vapor deposition of a silicon nitride layer at a pressure of at least 1 Torr, a temperature of less than 700° C. and using feed gases comprising a silicon hydride and ammonia; and
exposing the substrate with silicon nitride layer to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the silicon nitride layer, the providing of at least one of the semiconductive region and the transistor gate occurring after the exposing.

### Claim 51 (depends on 50)

The method of claim 50 wherein the silicon nitride layer is formed on an oxide layer constituting a portion of the gate dielectric layer.

### Claim 52 (depends on 50)

The method of claim 50 wherein the pressure during the forming of the silicon nitride is less than or equal to 2.5 Torr.

### Claim 53 (depends on 50)

The method of claim 50 wherein the temperature during the forming of the silicon nitride is less than or equal to 650° C.

### Claim 54 (depends on 50)

The method of claim 50 wherein the pressure during the forming of the silicon nitride is less than or equal to 2.5 Torr, and the temperature during the forming of the silicon nitride is less than or equal to 650° C.

### Claim 55 (depends on 50)

The method of claim 50 wherein the silicon nitride is formed to a thickness no greater than 60 Angstroms.

### Claim 56 (depends on 50)

The method of claim 50 wherein the transistor gate is provided in the form of a floating gate.

### Claim 57

A method of forming a transistor gate construction comprising:
providing a semiconductive region of a substrate to be gated;
providing a conductive transistor gate proximate the region to be gated;
providing a gate dielectric layer intermediate the region to be gated and the transistor gate, the gate dielectric layer being at least partially provided by forming a first silicon nitride layer by low pressure chemical vapor deposition using a first set of reactor conditions using feed gases comprising a silicon hydride and ammonia;
after using the first set of conditions, forming a second silicon nitride layer on the first silicon nitride layer by low pressure chemical vapor deposition using a second set of reactor conditions using feed gases comprising a silicon hydride and ammonia; and
exposing the substrate with first and second silicon nitride layers to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the second silicon nitride layer, the providing of at least one of the semiconductive region and the transistor gate occurring after the exposing.

### Claim 58 (depends on 57)

The method of claim 57 wherein the first silicon nitride layer is formed on an oxide layer constituting a portion of the gate dielectric layer.

### Claim 59 (depends on 57)

The method of claim 57 wherein the first and second silicon nitride layers are formed to provide a combined thickness of the first and second nitride layers of no greater than 60 Angstroms.

### Claim 60 (depends on 57)

The method of claim 57 wherein the transistor gate is provided in the form of a floating gate.

### Claim 61

A method of forming a transistor gate construction comprising:
providing a semiconductive region of a substrate to be gated;
providing a conductive transistor gate proximate the region to be gated;
providing a gate dielectric layer intermediate the region to be gated and the transistor gate, the gate dielectric layer being at least partially provided by first exposing the substrate to rapid thermal nitridation conditions effective to grow a seed nitride layer to a thickness of at least about 8 Angstroms;
forming a silicon nitride layer over the seed nitride layer by low pressure chemical vapor deposition at a pressure of less than 1 Torr, a temperature of at least 700° C. and using feed gases comprising a silicon hydride and ammonia; and
second exposing the substrate with silicon nitride layer to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the silicon nitride layer, the providing of at least one of the semiconductive region and the transistor gate occurring after the second exposing.

### Claim 62 (depends on 61)

The method of claim 61 wherein the seed nitride layer is formed on an oxide layer constituting a portion of the gate dielectric layer.

### Claim 63 (depends on 61)

The method of claim 61 wherein the seed layer is grown to a thickness of no greater than 20 Angstroms.

### Claim 64 (depends on 61)

The method of claim 61 wherein the transistor gate is provided in the form of a floating gate.

### Claim 65

A method of forming a transistor gate construction comprising:
providing a semiconductive region of a substrate to be gated;
providing a conductive transistor gate proximate the region to be gated;
providing a gate dielectric layer intermediate the region to be gated and the transistor gate, the gate dielectric layer being at least partially provided by first exposing the substrate to rapid thermal nitridation conditions effective to grow a seed nitride layer to a thickness of at least about 8 Angstroms;
forming a silicon nitride layer over the seed nitride layer by low pressure chemical vapor deposition at a pressure of at least 1 Torr, a temperature of less than 700° C. and using feed gases comprising a silicon hydride and ammonia; and
second exposing the substrate with silicon nitride layer to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the silicon nitride layer, the providing of at least one of the semiconductive region and the transistor gate occurring after the second exposing.

### Claim 66 (depends on 65)

The method of claim 65 wherein the seed nitride layer is formed on an oxide layer constituting a portion of the gate dielectric layer.

### Claim 67 (depends on 65)

The method of claim 65 wherein the seed layer is grown to a thickness of no greater than 20 Angstroms.

### Claim 68 (depends on 65)

The method of claim 65 wherein the transistor gate is provided in the form of a floating gate.

### Claim 69

A method of forming a transistor gate construction comprising:
providing a semiconductive region of a substrate to be gated;
providing a conductive transistor gate proximate the region to be gated;
providing a gate dielectric layer intermediate the region to be gated and the transistor gate, the gate dielectric layer being at least partially provided by low pressure chemical vapor deposition of a silicon nitride layer using feed gases comprising a silicon hydride and ammonia;
after forming the silicon nitride layer, exposing the substrate to a nitrogen containing atmosphere which is substantially void of silicon hydride at a temperature of at least about 850° C.; and
after exposing the substrate to the nitrogen containing atmosphere, exposing the substrate with silicon nitride layer to oxidizing conditions comprising at least 700° C. to form a silicon dioxide layer over the silicon nitride layer, the providing of at least one of the semiconductive region and the transistor gate occurring after the exposing to said oxidizing conditions.

### Claim 70 (depends on 69)

The method of claim 69 wherein the silicon nitride layer is formed on an oxide layer constituting a portion of the gate dielectric layer.

### Claim 71 (depends on 69)

The method of claim 69 wherein the nitrogen containing atmosphere comprises ammonia.

### Claim 72 (depends on 69)

The method of claim 69 wherein the nitrogen containing atmosphere comprises an oxynitride compound.

### Claim 73 (depends on 69)

The method of claim 69 wherein the transistor gate is provided in the form of a floating gate.

### Claim 74

A method of forming an electronic device incorporating a high K dielectric layer construction comprising:
forming and high K dielectric layer over a substrate;
low pressure chemical vapor depositing a silicon nitride layer on the high K dielectric layer at a pressure of at least 1 Torr, a temperature of less than 700° C. and using feed gases comprising a silicon hydride and ammonia; and
forming a conductive component on the silicon nitride layer.

### Claim 75

A method of forming an electronic device incorporating a high K dielectric layer construction comprising:
forming and high K dielectric layer over a substrate;
low pressure chemical vapor depositing a first nitride layer on the high K dielectric layer using a first set of reactor conditions using feed gases comprising a silicon hydride and ammonia;
after using the first set of conditions, forming a second silicon nitride layer on the first silicon nitride layer by low pressure chemical vapor deposition using a second set of reactor conditions using feed gases comprising a silicon hydride and ammonia; and
forming a conductive component on the second silicon nitride layer.

### Claim 76

A method of forming an electronic device incorporating a high K dielectric layer construction comprising:
forming and high K dielectric layer over a substrate;
first exposing the high K dielectric layer to rapid thermal nitridation conditions effective to grow a seed nitride layer to a thickness of at least about 8 Angstroms on the high K dielectric layer;
forming a silicon nitride layer over the seed nitride layer by low pressure chemical vapor deposition at a pressure of less than 1 Torr, a temperature of at least 700° C. and using feed gases comprising a silicon hydride and ammonia; and
forming a conductive component on the silicon nitride layer.

### Claim 77

A method of forming an electronic device incorporating a high K dielectric layer construction comprising:
forming and high K dielectric layer over a substrate;
first exposing the high K dielectric layer to rapid thermal nitridation conditions effective to grow a seed nitride layer to a thickness of at least about 8 Angstroms on the high K dielectric layer;
forming a silicon nitride layer over the seed nitride layer by low pressure chemical vapor deposition at a pressure of at least 1 Torr, a temperature of less than 700° C. and using feed gases comprising a silicon hydride and ammonia; and
forming a conductive component on the silicon nitride layer.

### Claim 78

A method of forming an electronic device incorporating a high K dielectric layer construction comprising:
forming and high K dielectric layer over a substrate;
low pressure chemical vapor depositing a silicon nitride layer on the high K dielectric layer using feed gases comprising a silicon hydride and ammonia;
after forming the silicon nitride layer, exposing the substrate to a nitrogen containing atmosphere which is substantially void of silicon hydride at a temperature of at least about 850° C.; and
after the exposing, forming a conductive component on the silicon nitride layer.