# US 2001/0023726 A1 · Fabrication and bonding of copper sputter targets

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2001/0023726 A1
- Document ID: US20010023726A1
- Status: Published application
- Kind: A1
- Application number: 09/730,349
- Filed: 2000-12-05
- Published: 2001-09-27
- Earliest claimed: 1999-07-08
- Assignees: Praxair S.T. Technology, Inc.
- Inventors: Holger Koenigsmann; Alfred Snowman; Shailesh Kulkarni
- Web page: https://patentgrep.com/patent/US20010023726A1

## CPC

- C22F 1/08: of copper or alloys based thereon
- C23C 14/3414: {Metallurgical or chemical aspects of target preparation, e.g. casting, powder metallurgy}
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

The method is used to fabricate pure copper sputter targets. It includes first heating a copper billet to a temperature of at least 500° C. The copper billet has a purity of at least 99.99 percent. Then warm working the copper billet applies at least 40 percent strain. Cold rolling the warm worked copper billet then applies at least 40 percent strain and forms a copper plate. Finally, annealing the copper plate at a temperature above about 250° C. forms a target blank. The target blank has equiaxed grains having an average grain size of less than 40 μm. The grains of the target blank have (111), (200), (220) and (311) orientations with the amount of the grains having each of the orientations being less than 50 percent.

## Claims

### Claim 1

A method of fabricating copper sputter targets comprising the steps of:
heating a copper billet to at least about 500° C., the copper billet having a purity of at least 99.99 percent;
warm working the heated copper billet to apply at least about 40 percent strain;
cold rolling the warm worked copper billet to apply at least about 40 percent strain and to form a copper plate; and
annealing the copper plate at a temperature above about 250° C. to form a target blank, the target blank having equiaxed grains, the grains having an average grain size of less than about 40 μm and having (111), (200), (220) and (311) orientations with the amount of the grains having each of the orientations being less than about 50 percent.

### Claim 2 (depends on 1)

The method of claim 1, wherein the copper billet is heated to a temperature between about 500 and 750° C.

### Claim 3 (depends on 1)

The method of claim 1, wherein the warm working introduces about 40 to 80 percent strain into the copper billet.

### Claim 4 (depends on 3)

The method of claim 3, wherein the warm working is a technique selected from the group consisting of: pressing, forging, equi-channel angular extrusion and rolling.

### Claim 5 (depends on 1)

The method of claim 1, wherein the cold rolling introduces between about 40 and 80 percent strain into the copper plate.

### Claim 6 (depends on 1)

The method of claim 1, wherein the annealing occurs at a temperature between about 250 and 400° C.

### Claim 7

A method of fabricating copper sputter targets comprising the steps of:
heating a copper billet to a temperature between about 500 and 750° C., the copper billet having a purity of at least 99.999 percent;
warm working the heated copper billet to between about 40 and 80 percent strain;
cold rolling the warm worked copper billet to apply between about 40 and 80 percent strain and to form a copper plate; and
annealing the copper plate at a temperature between about 250 and 400° C. to form a target blank, the target blank having equiaxed grains, the grains having an average grain size between about 10 and 35 μm and having (111), (200), (220) and (311) orientations with the amount of the grains having each of the orientations being less than about 50 percent.

### Claim 8 (depends on 7)

The method of claim 7, wherein the copper billet is heated to a temperature between about 600 and 700° C.

### Claim 9 (depends on 7)

The method of claim 7, wherein the warm working introduces about 50 to 70 percent strain into the copper billet.

### Claim 10 (depends on 9)

The method of claim 9, wherein the warm working is a technique selected from the group consisting of: pressing, forging, equi-channel angular extrusion and rolling.

### Claim 11 (depends on 7)

The method of claim 7, wherein the cold rolling introduces between about 50 and 70 percent strain into the copper plate.

### Claim 12 (depends on 7)

The method of claim 7, wherein the annealing occurs at a temperature between about 300 and 375° C.

### Claim 13

A method of fabricating copper sputter targets comprising the steps of:
heating a copper billet to a temperature between about 600 and 700° C., the copper billet having a purity of at least 99.999 percent;
warm working the heated copper billet to between about 50 and 70 percent strain, the heated billet having a temperature between about 600 and 700° C.;
cold rolling the warm worked copper billet to apply between about 50 and 70 percent strain and to form a copper plate; and
annealing the copper plate at a temperature between about 300 and 375° C. to form a target blank, the target blank having an average grain size of between about 10 and 30 μm and the target blank containing grains having the (111), (200), (220) and (311) orientations with the amount of the grains having each of the orientations being less than about 50 percent.

### Claim 14 (depends on 13)

The method of claim 13, wherein the warm working is pressing.

### Claim 15 (depends on 13)

The method of claim 13, wherein the amount of grains with the (111), (200), (220) and (311) orientations is between about 15 and 35 percent.

### Claim 16 (depends on 13)

The method of claim 13, including the additional steps of:
flattening the target blank at the elevated temperature; and
explosion bonding the target blank to a backing plate.

### Claim 17 (depends on 1)