# US 2001/0023721 A1 · Damage tolerant aluminum alloy product and method of its manufacture

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2001/0023721 A1
- Document ID: US20010023721A1
- Status: Published application
- Kind: A1
- Application number: 09/845,181
- Filed: 2001-05-01
- Published: 2001-09-27
- Earliest claimed: 1998-12-22
- Inventors: Alfred Ludwig Heinz; Alfred Johann Peter Haszler
- Web page: https://patentgrep.com/patent/US20010023721A1

## CPC

- B32B 15/016: {all layers being formed of aluminium or aluminium alloys}
- C22C 21/16: with magnesium
- C22F 1/057: of alloys with copper as the next major constituent
- Y10T 428/12764: Next to Al-base component
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

The invention relates to a product comprising an aluminum base alloy consisting of (in weight %): Cu 3.8 - 4.9, Mg 1.2 - 1.8, Mn 0.1 - 0.9, Fe max. 0.12, Si max. 0.10, Ti max. 0.15, Zn max. 0.20, Cr max. 0.10, impurities each max. 0.05, total max. 0.15, balance aluminum. The product having a minimum L-0.2% yield strength of 300 MPa or more, a minimum LT-0.2% yield strength of 270 MPa, a minimum T-L fracture toughness KC(ao) of 100 MPa.{square root}m or more for a 700 mm wide CCT-panel, and has in both L/ST- and LT/ST-sections an average grain size of at least 6 according to ASTM E-112. Further the invention relates to a method for the manufacturing of such a product.

## Claims

### Claim 1

A damage tolerant alloy product comprising an aluminum base alloy consisting essentially of (in weight %): 10 Cu 3.8-4.9 Mg 1.2-1.8 Mn 0.1-0.9 Fe max. 0.12 Si max. 0.10 Ti max. 0.15 Zn max. 0.20 Cr max. 0.10 impurities each max. 0.05 total max. 0.15
balance aluminum,
said product having a minimum L-0.2% yield strength of 300 MPa or more, a minimum LT-0.2% yield strength of 270 MPa, a minimum T-L fracture toughness KC(ao) of 100 MPa.{square root}m or more for a 700 mm wide CCT-panel, and having in both L/ST- and LT/ST-sections an average grain size of at least 6 according to ASTM E-112.

### Claim 2 (depends on 1)

The product in accordance with claim 1, wherein the Cu content is in a range of 3.8 to 4.7%.

### Claim 3 (depends on 1)

The product in accordance with claim 1, wherein the Cu content is in a range of 3.9 to 4.6%.

### Claim 4 (depends on 1)

The product in accordance with claim 1, wherein the Mg content is in a range of 1.2 to 1.7%.

### Claim 5 (depends on 1)

The product in accordance with claim 1, wherein the Mn content is in a range of 0.1 to 0.8%.

### Claim 6 (depends on 1)

The product in accordance with claim 1, wherein the product has minimum longitudinal (L)-0.2% yield strength of 360 MPa or more, the minimum 0.2% yield strength in the TL-direction (transverse direction) is 300 MPa.

### Claim 7 (depends on 1)

The product in accordance with claim 1, wherein the product has minimum transverse (TL)-tensile strength of 440 MPa or more and a minimum longitudinal (L)-tensile strength of 475 MPa or more.

### Claim 8 (depends on 1)

The product in accordance with claim 1, wherein the product has minimum L-T fracture toughness KC(ao) of 105 MPa.{square root}m for 700 mm wide CCT-panels.

### Claim 9 (depends on 1)

The product in accordance with claim 1, wherein the minimum T-L fracture toughness KC(ao) is 170 MPa.{square root}m or more for 2000 mm wide CCT-panels.

### Claim 10 (depends on 1)

The product in accordance with claim 1, wherein the minimum T-L fracture toughness KC(ao) is 175 MPa.{square root}m or more for 2000 mm wide CCT-panels.

### Claim 11 (depends on 1)

The product in accordance with claim 1, wherein the grain aspect ratio in both L/ST- and LT/ST-sections is 1:4 or less.

### Claim 12 (depends on 1)

The product in accordance with claim 1, wherein the grain aspect ratio in both L/ST- and LT/ST-sections is 1:3 or less.

### Claim 13 (depends on 1)

The product in accordance with claim 1, wherein the grain aspect ratio in both L/ST- and LT/ST-sections is 1:2 or less.

### Claim 14 (depends on 1)

The product in accordance with claim 1, wherein the product is a sheet product.

### Claim 15 (depends on 1)

The product in accordance with any one of claim 1, wherein the product is a plate product.

### Claim 16 (depends on 1)

A composite comprising the product in accordance with claim 1, and a cladding on the product, the cladding comprising a higher purity aluminum alloy than said product.

### Claim 17 (depends on 1)

A composite comprising the product in accordance with claim 1, and a cladding on the product, the cladding comprising a member of the group consisting of:
(i) an alloy of the Aluminum Association AA1000 series;
(ii) an alloy of the Aluminum Association AA6000 series; and
(iii) an alloy of the Aluminum Association AA7000 series.

### Claim 18

A method for manufacturing a damage tolerant alloy product, comprising the steps of:
(a) casting an ingot or a slab comprising an aluminum alloy consisting of (in wt. %): 11 Cu 3.8-4.9 Mg 1.2-1.8 Mn 0.1-0.9 Fe max. 0.12 Si max. 0.10 Ti max. 0.15 Zn max. 0.20 Cr max. 0.10 impurities each max. 0.05 total max. 0.15
balance aluminum;
(b) hot rolling the ingot to form an intermediate product;
(c) cold rolling the intermediate product to form a rolled product in both the length and in the width direction with a total cold deformation of more than 60%;
(d) solution heat treating the intermediate product after cold rolling in at least one direction;
(e) cooling the solution heat treated intermediate product; and
(f) ageing the cooled intermediate product;
said damage tolerant product having a minimum L-0.2% yield strength of 300 MPa or more, a minimum LT-0.2% yield strength of 270 MPa, a minimum T-L fracture toughness KC(ao) of 100 MPa.{square root}m or more for a 700 mm wide CCT-panel, and having in both L/ST- and LT/ST-sections an average grain size of at least 6 according to ASTM E-112.

### Claim 19 (depends on 18)

The method in accordance with claim 18, wherein during step (b) the ingot is hot rolled in both the length and in the width direction.

### Claim 20 (depends on 18)

The method in accordance with claim 18, wherein during step (c) the intermediate product is first cold rolled in the one direction with a total cold deformation in the range of 20 to 55% and then further cold rolled in the other direction to a rolled product with a total cold deformation of 60% or more.

### Claim 21 (depends on 20)

The method in accordance with claim 20, wherein the process step (c) comprises the sequential steps of:
(c-i) first cold rolling the intermediate product in one direction with a total cold deformation in the range of 20 to 55%;
(c-ii) solution heat treating the intermediate product after cold rolling;
(c-iii) tempering the solution heat treated intermediate product to a T3 or a T351-temper;
(c-iv) soft annealing the tempered intermediate product; and
(c-v) cold rolling of the soft annealed intermediate product in at least another direction to a final gauge thickness with a total cold deformation of more than 60%.

### Claim 22 (depends on 21)

The method in accordance with claim 21, wherein during process step (c-v) the soft annealed intermediate product is being cold rolled in both the length and in the width direction.

### Claim 23 (depends on 21)

The method in accordance with claim 21, wherein the hot rolling of the ingot to the intermediate product occurs after homogenization at a temperature of 400 to 505° C.

### Claim 24 (depends on 21)

The method in accordance with claim 21, wherein solution heat treating of the intermediate product after cold rolling in at least one direction occurs at a temperature of 460 to 505° C. for 5 to 120 minutes.

### Claim 24 (depends on 21)

The method in accordance with claim 21, wherein the solution heat treated intermediate product is cooled to a temperature of 175° C. or lower.

### Claim 25 (depends on 21)

The method in accordance with claim 21, wherein soft annealing of the cooled intermediate product occurs at a temperature of 300 to 430° C. for 0.5 to 12 hours.

### Claim 26 (depends on 21)

The method in accordance with claim 21, wherein between cold rolling passes, the intermediate product is inter-annealed at a temperature of 300 to 430° C. for 0.5 to 12 hours.

### Claim 27 (depends on 1)

An aircraft skin comprising a sheet or plate of the damage tolerant alloy product of claim 1.

### Claim 28 (depends on 18)

An aircraft skin comprising a sheet or plate of the damage tolerant alloy product made by the method of claim 18.

### Claim 29

A damage tolerant alloy product comprising an aluminum base alloy consisting of (in weight %): 12 Cu 3.8-4.9 Mg 1.2-1.8 Mn 0.1-0.9 Fe max. 0.12 Si max. 0.10 Ti max. 0.15 Zn max. 0.20 Cr max. 0.10 impurities each max. 0.05 total max. 0.15
balance aluminum,
said product having a minimum L-0.2% yield strength of 300 MPa or more, a minimum LT-0.2% yield strength of 270 MPa, a minimum T-L fracture toughness KC(ao) of 100 MPa.{square root}m or more for a 700 mm wide CCT-panel, and having in both L/ST- and LT/ST-sections an average grain size of at least 6 according to ASTM E-112.