# US 2001/0011066 A1 · Fabrication of superconducting wires and rods

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 2001/0011066 A1
- Document ID: US20010011066A1
- Status: Published application
- Kind: A1
- Application number: 09/766,451
- Filed: 2001-01-19
- Published: 2001-08-02
- Earliest claimed: 1995-01-13
- Assignees: University of Houston
- Inventors: Krishnaswamy Ravi-Chandar; Devamanohar Ponnusamy; Kamel Salama
- Web page: https://patentgrep.com/patent/US20010011066A1

## CPC

- H10N 60/0801: {Manufacture or treatment of filaments or composite wires}
- Y10S 505/74: To form wire or fiber
- Y10T 29/49014: Superconductor
- H10N: ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- Y10S: TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
- Y10T: TECHNICAL SUBJECTS COVERED BY FORMER US CLASSIFICATION

## Abstract

The fabrication of superconducting wires and rods having desired and consistent electrical and mechanical properties, in particular those based on Yttrium Barium Copper Oxide (YBCO) and Bismuth Strontium Calcium Copper Oxide (BSCCO), is disclosed. The first fabrication step is to form an extrudable paste by mixing YBCO or BSCCO superconducting powder with a set of organic additives, which include binder, plasticizers lubricant, dispersant, and a solvent. The following additional steps are performed on both YBCO and BSCCO based wires or rods: (i) using a piston extruder to extrude the superconducting wire or rod; (ii) drying the wire or rod to remove the solvent; and (iii) subjecting the wire or rod to a binder burn-out treatment to remove the remaining organic additives. In addition, YBCO wires and rods also require a sintering step, while BSCCO wires and rods also require cold isostatic pressing and heat treatment steps. The formation of cracks in thicker YBCO and BSCCO based rods during the drying and heating process steps is avoided by extruding hollow rods. The additives, processing parameters, and processing stages used to fabricate the superconducting wires and rods help achieve desired and consistent electrical and mechanical properties.

## Claims

### Claim 1

An extrudable paste used in the fabrication of superconducting wires and rods, comprising:
(a) a superconducting powder;
(b) ethyl cellulose;
(c) glycerol;
(d) stearic acid;
(e) triolein; and
(f) a solvent.

### Claim 2 (depends on 1)

The extrudable paste of claim 1, wherein said superconducting powder is YBCO or BSCCO.

### Claim 3 (depends on 1)

The extrudable paste of claim 1, wherein said solvent is butyl carbitol, ethyl alcohol, or a mixture of butyl carbitol and ethyl alcohol.

### Claim 4 (depends on 3)

The extrudable paste of claim 3, wherein said superconducting powder is YBCO or BSCCO.

### Claim 5 (depends on 1)

The extrudable paste of claim 1, wherein said superconducting powder consists of particles having sizes of about 2 to 10 μm.

### Claim 6 (depends on 2)

The extrudable paste of claim 2, wherein said superconducting powder consists of particles having sizes of about 2 to 10 μm.

### Claim 7 (depends on 3)

The extrudable paste of claim 3, wherein said superconducting powder consists of particles having sizes of about 2 to 10 μm.

### Claim 8 (depends on 4)

The extrudable paste of claim 4, wherein said superconducting powder consists of particles having sizes of about 2 to 10 μm.

### Claim 9

An extrudable paste used in the fabrication of superconducting wire, comprising:
(a) superconducting powder;
(b) about 2 to 3 weight percent of ethyl cellulose;
(c) about 0.7 to 0.75 weight percent of glycerol;
(d) about 0.4 to 0.5 weight percent of stearic acid;
(e) about 0.1 weight percent of triolein; and
(f) about 15 to 18 weight percent of solvent.

### Claim 10 (depends on 9)

The extrudable paste of claim 9, wherein said superconducting powder is YBCO or BSCCO.

### Claim 11 (depends on 9)

The extrudable paste of claim 9, wherein said solvent is butyl carbitol, ethyl alcohol, or a mixture of butyl carbitol and ethyl alcohol.

### Claim 12 (depends on 11)

The extrudable paste of claim 11, wherein said superconducting powder is YBCO or BSCCO.

### Claim 13 (depends on 9)

The extrudable paste of claim 9, wherein said superconducting powder consists of particles having sizes of about 2 to 10 μm.

### Claim 14 (depends on 10)

The extrudable paste of claim 10, wherein said superconducting powder consists of particles having sizes of about 2 to 10 μm.

### Claim 15 (depends on 11)

The extrudable paste of claim 11, wherein said superconducting powder consists of particles having sizes of about 2 to 10 μm.

### Claim 16 (depends on 12)

The extrudable paste of claim 12, wherein said superconducting powder consists of particles having sizes of about 2 to 10 μm.

### Claim 17

An extrusion process for extruding superconducting wires and rods, comprising the steps of:
(a) providing a piston extruder comprising a die barrel, an extrusion nozzle, and a ram;
(b) closing said extrusion nozzle;
(c) loading extrudable paste in the form of granules into said die barrel, said extrudable paste comprising superconducting powder, a binder, a plasticizer, a lubricant, a dispersant, and a solvent;
(d) subjecting said die barrel to a vacuum of about 200 millitorr;
(e) compacting said extrudable paste by using said ram to apply a compaction stress of about 100 MPa;
(f) opening said extrusion nozzle; and
(g) extruding a wire or rod through said extrusion nozzle using said ram, said ram moving at a rate of about 0.02 to 0.1 inch/minute.

### Claim 18 (depends on 17)

The extrusion process of claim 17, further comprising the step of forming a hollow rod by attaching a mandrel to said ram.

### Claim 19 (depends on 17)

The extrusion process of claim 17, wherein said granules of extrudable paste are cubes having sides measuring about 2 to 3 mm.

### Claim 20 (depends on 18)

The extrusion process of claim 18, wherein said granules of extrudable paste are cubes having sides measuring about 2 to 3 mm.

### Claim 21 (depends on 17)

The extrusion process of claim 17, wherein said dispersant is triolein.

### Claim 22 (depends on 18)

The extrusion process of claim 18, wherein said dispersant is triolein.

### Claim 23 (depends on 19)

The extrusion process of claim 19, wherein said dispersant is triolein.

### Claim 24 (depends on 20)

The extrusion process of claim 20, wherein said dispersant is triolein.

### Claim 25

A method of drying a superconducting wire or rod, comprising the steps of:
(a) providing a superconducting wire or rod comprising at least superconducting powder, and a solvent;
(b) initially drying said wire or rod in still air at room temperature until about 20% of said solvent is removed; and
(c) subsequently drying said wire or rod in flowing air at a temperature of about 60° C. until all remaining solvent is removed.

### Claim 26 (depends on 17)

The extrusion process of claim 17, further comprising the steps of:
initially drying said wire or rod in still air at room temperature until about 20% of said solvent is removed; and
subsequently drying said wire or rod in flowing air at a temperature of about 60° C. until all remaining solvent is removed.

### Claim 27 (depends on 26)

The extrusion process of claim 26, further comprising the step of forming a hollow rod by attaching a mandrel to said ram.

### Claim 28

A method of removing organic additives from a superconducting wire or rod, comprising the steps of:
(a) providing a superconducting wire or rod comprising at least superconducting powder and organic additives;
(b) initially heating said wire or rod in flowing oxygen until a temperature of about 100° C. is reached;
(c) subsequently heating said wire or rod in flowing oxygen at a rate in the range of about 6 to 15° C./hour until a temperature of about 300° C. is reached; and
(d) thereafter heating said wire or rod in flowing oxygen at a rate of about 20° C./hour until a temperature of about 500° C. is reached.

### Claim 29 (depends on 28)

The method of claim 28, wherein in the temperature range of about 100 to 300° C., if said wire or rod has a diameter less than about 2 mm, said wire or rod is heated, in flowing oxygen, at a rate of about 15° C./hour, while if said wire or rod has a diameter equal to or greater than about 2 mm, said wire or rod is heated, in flowing oxygen, at a rate of about 6° C./hour.

### Claim 30 (depends on 28)

The method of claim 28, wherein said flowing oxygen has a flow rate of about 2 liters per minute for about 100 grams of said wire or rod being heated to a temperature of about 300° C., and a flow rate of about an additional 2 liters per minute for each additional 100 grams of said wire or rod being heated to about 300° C., and wherein said flowing oxygen has a flow rate of about 0.25 liters per minute for about 100 grams of said wire or rod being heated at a temperature above about 300° C., and a flow rate of about an additional 0.25 liters per minute for each additional 100 grams of said wire or rod heated about 300° C.

### Claim 31 (depends on 26)

The extrusion process of claim 26, further comprising the steps of:
initially heating said wire or rod in flowing oxygen until a temperature of about 100° C. is reached;
subsequently heating said wire or rod in flowing oxygen at a rate in the range of about 6 to 15° C./hour until a temperature of about 300° C. is reached; and
thereafter heating said wire or rod in flowing oxygen at a rate of about 20° C./hour until a temperature of about 500° C. is reached.

### Claim 32 (depends on 31)

The extrusion process of claim 31, further comprising the step of forming a hollow rod by attaching a mandrel to said ram.

### Claim 33

A process for fabricating superconducting wires and rods, comprising the steps of:
(a) providing a piston extruder comprising a die barrel, an extrusion nozzle, and a ram;
(b) closing said extrusion nozzle;
(c) loading extrudable paste in the form of granules into said die barrel, said extrudable paste comprising YBCO powder, a binder, a plasticizer, a lubricant, a dispersant, and a solvent;
(d) subjecting said die barrel to a vacuum of about 200 millitorr;
(e) compacting said extrudable paste by using said ram to apply a compaction stress of about 100 MPa;
(f) opening said extrusion nozzle;
(g) extruding a wire or rod through said extrusion nozzle using said ram, said ram extruding said wire or rod at a rate of about 0.02 to 0.1 inch/minute;
(h) initially drying said wire or rod in still air at room temperature until about 20% of said solvent is removed;
(i) subsequently drying said wire or rod in flowing air at a temperature of about 60° C. until all remaining solvent is removed;
(j) initially heating said wire or rod in flowing oxygen until a temperature of about 100° C. is reached;
(k) subsequently heating said wire or rod in flowing oxygen at a rate in the range of about 6 to 15° C./hour until a temperature of about 300° C. is reached;
(l) thereafter heating said wire or rod in flowing oxygen at a rate of about 20° C./hour until a temperature of about 500° C. is reached; and
(m) sintering said wire or rod at about 900° C. in an oxygen atmosphere for about 24 hours.

### Claim 34 (depends on 33)

The extrusion process of claim 33, further comprising the step of forming a hollow rod by attaching a mandrel to said ram.

### Claim 35 (depends on 33)

The process of claim 33, wherein said dispersant is-triolein.

### Claim 36 (depends on 33)

The process of claim 33, further comprising the step of exposing said wire or rod to an oxygen atmosphere at a temperature of about 500° C. for about 24 hours.

### Claim 37

A method of achieving a highly oriented, polycrystalline microstructure in superconducting wires or rods, comprising the steps of:
(a) providing a superconducting wire or rod;
(b) packing said wire or rod in a flexible container;
(c) placing said container in a support fixture;
(d) applying a first isostatic load to said container to densify said wire or rod;
(e) heating said wire or rod, in an atmosphere of about 9% oxygen and about 91% argon, at a temperature of about 830° C. for about 72 hours;
(f) applying a second isostatic load to said container to densify said wire or rod; and
(g) heating said wire or rod, in an atmosphere of about 9% oxygen and about 91% argon at 840° C. for about 72 hours.

### Claim 38 (depends on 37)

The method of claim 37, wherein said superconducting wires or rods comprise BSCCO.

### Claim 39 (depends on 37)

The method of claim 37, wherein said first isostatic load is about 40 Ksi, and said second isostatic load is about 60 Ksi.

### Claim 40 (depends on 38)

The method of claim 38, wherein said first isostatic load is about 40 Ksi, and said second isostatic load is about 60 Ksi.

### Claim 41 (depends on 37)

The method of claim 37, wherein if said superconducting wire or rod has a hollow center, further comprising the step of inserting a mandrel or rod into said hollow center prior to applying an isostatic load to said wire or rod.

### Claim 42

A process for fabricating superconducting wires and rods, comprising the steps of:
(a) providing a piston extruder comprising a die barrel, an extrusion nozzle, and a ram;
(b) closing said extrusion nozzle;
(c) loading extrudable paste in the form of granules into said die barrel, said extrudable paste comprising BSCCO powder, a binder, a plasticizer, a lubricant, a dispersant, and a solvent;
(d) subjecting said die barrel to a vacuum of about 200 millitorr;
(e) compacting said extrudable paste by using said ram to apply a compaction stress of about 100 MPa;
(f) opening said extrusion nozzle;
(g) extruding a wire or rod through said extrusion nozzle using said ram, said ram extruding said wire or rod at a rate of about 0.02 to 0.1 inch/minute;
(h) initially drying said wire or rod in still air at room temperature until about 20% of said solvent is removed;
(i) subsequently drying said wire or rod in flowing air at a temperature of about 60° C. until all remaining solvent is removed;
(j) initially heating said wire or rod in flowing oxygen until a temperature of about 100° C. is reached;
(k) subsequently heating said wire or rod in flowing oxygen at a rate in the range of about 6 to 15° C./hour until a temperature of about 300° C. is reached;
(l) thereafter heating said wire or rod in flowing oxygen at a rate of about 20° C./hour until a temperature of about 500° C. is reached;
(m) packing said wire or rod in a flexible container;
(n) placing said container in a support fixture;
(o) applying a first isostatic load to said container to densify said wire or rod;
(p) heating said wire or rod, in an atmosphere of about 9% oxygen and about 91% argon, at a temperature of about 830° C. for about 72 hours;
(q) applying a second isostatic load to said container to densify said wire or rod; and
(r) heating said wire or rod, in an atmosphere of about 9% oxygen and about 91% argon at about 840° C. for about 72 hours.

### Claim 43 (depends on 42)

The process of claim 42, wherein a mandrel is attached to said ram to form a wire or rod with a hollow center, and further comprising the step of inserting a mandrel or rod into said hollow center prior to applying an isostatic load to said wire or rod.

### Claim 44 (depends on 42)

The process of claim 42, wherein said dispersant is triolein.

### Claim 45

A superconducting wire or rod which is extruded by the steps of:
(a) providing a piston extruder comprising a die barrel, an extrusion nozzle, and a ram;
(b) closing said extrusion nozzle;
(c) loading extrudable paste in the form of granules into said die barrel, said extrudable paste comprising superconducting powder, a binder, a plasticizer, a lubricant, a dispersant, and a solvent;
(d) subjecting said die barrel to a vacuum of about 200 millitorr;
(e) compacting said extrudable paste By using said ram to apply a compaction stress of about 100 MPa;
(f) opening said extrusion nozzle; and
(g) extruding a wire: or rod through said extrusion nozzle using said ram, said ram moving at a rate of about 0.02 to 0.1 inch/minute.

### Claim 46 (depends on 45)

The superconducting wire or rod of claim 45, wherein said granules of extrudable paste are cubes having sides measuring about 2 to 3 mm.

### Claim 47 (depends on 45)

The superconducting wire or rod of claim 45, wherein said dispersant is triolein.

### Claim 48

A hollow superconducting wire or rod which is extruded by the steps of:
(a) providing a piston extruder comprising a die barrel, an extrusion nozzle, and a ram having a mandrel attached;
(b) closing said extrusion nozzle;
(c) loading extrudable paste in the form of granules into said die barrel, said extrudable paste comprising superconducting powder, a binder, a plasticizer, a lubricant, a dispersant, and a solvent;
(d) subjecting said die barrel to a vacuum of about 200 millitorr;
(e) compacting said extrudable paste by using said ram to apply a compaction stress of about 100 MPa;
(f) opening said extrusion nozzle; and
(g) extruding a hollow wire or rod through said extrusion nozzle using said ram, said ram moving at a rate of about 0.02 to 0.1 inch/minute.

### Claim 49 (depends on 48)

The hollow superconducting wire or rod of claim 48, wherein said granules of extrudable paste are cubes having sides measuring about 2 to 3 mm.

### Claim 50 (depends on 48)

The hollow superconducting wire or rod of claim 48, wherein said dispersant is triolein.

### Claim 51

A superconducting wire or rod which is fabricated by the steps of:
(a) providing a piston extruder comprising a die barrel, an extrusion nozzle, and a ram;
(b) closing said extrusion nozzle;
(c) loading extrudable paste in the form of granules into said die barrel, said extrudable paste comprising YBCO powder, a binder, a plasticizer, a lubricant, a dispersant, and a solvent;
(d) subjecting said die barrel to a vacuum of about 200 millitorr;
(e) compacting said extrudable paste by using said ram to apply a compaction stress of about 100 MPa;
(f) opening said extrusion nozzle;
(g) extruding a wire or rod through said extrusion nozzle using said ram, said ram extruding said wire or rod at a rate of about 0.02 to 0.1 inch/minute;
(h) initially drying said wire or rod in still air at room temperature until about 20% of said solvent is removed;
(i) subsequently drying said wire or rod in flowing air at a temperature of about 60° C. until all remaining solvent is removed;
(j) initially heating said wire or rod in flowing oxygen until a temperature of about 100° C. is reached;
(k) subsequently heating said wire or rod in flowing oxygen at a rate in the range of about 6 to 15° C./hour until a temperature of about 300° C. is reached;
(l) thereafter heating said wire or rod in flowing oxygen at a rate of about 20° C./hour until a temperature of about 500° C. is reached; and
(m) sintering said wire or rod at about 900° C. in an oxygen atmosphere for about 24 hours.

### Claim 52 (depends on 51)

The superconducting wire or rod of claim 51, wherein said wire or rod is fabricated in a hollow form by attaching a mandrel to said ram.

### Claim 53 (depends on 51)

The superconducting wire or rod of claim 51, wherein said dispersant is triolein.

### Claim 54 (depends on 51)

The superconducting wire or rod of claim 51, further comprising the fabrication step of exposing said wire or rod to an oxygen atmosphere at a temperature of about 500° C. for about 24 hours.

### Claim 55

A superconducting wire or rod which is fabricated by the steps of:
(a) providing a piston extruder comprising a die barrel, an extrusion nozzle, and a ram;
(b) closing said extrusion nozzle;
(c) loading extrudable paste in the form of granules into said die barrel, said extrudable paste comprising BSCCO powder, a binder, a plasticizer, a lubricant, a dispersant, and a solvent;,
(d) subjecting said die barrel to a vacuum of about 200 millitorr;
(e) compacting said extrudable paste by using said ram to apply a compaction stress of about 100 MPa;
(f) opening said extrusion nozzle;
(g) extruding a wire or rod through said extrusion nozzle using said ram, said ram extruding said wire or rod at a rate of about 0.02 to 0.1 inch/minute;
(h) initially drying said wire or rod in still air at room temperature until about 20% of said solvent is removed;
(i) subsequently drying said wire or rod in flowing air at a temperature of about 60° C. until all remaining solvent is removed;
(j) initially heating said wire or rod in flowing oxygen until a temperature of about 100° C. is reached;
(k) subsequently heating said wire or rod in flowing oxygen at a rate in the range of about 6 to 15° C./hour until a temperature of about 300° C. is reached;
(l) thereafter heating said wire or rod in flowing oxygen at a rate of about 20° C./hour until a temperature of about 500° C. is reached;
(m) packing said wire or rod in a flexible container;
(n) placing said container in a support fixture;
(o) applying a first isostatic load to said container to density said wire or rod;
(p) heating said wire or rod, in an atmosphere of about 9% oxygen and about 91% argon, at a temperature of about 830° C. for about 72 hours;
(q) applying a second isostatic load to said container to density said wire or rod; and
(r) heating said wire or rod, in an atmosphere of about 9% oxygen and about 91% argon at about 840° C. for about 72 hours.

### Claim 56 (depends on 55)

The superconducting wire or rod of claim 55, wherein said wire or rod is fabricated with a hollow center by attaching a mandrel to said ram, and further comprising the step of inserting a mandrel or rod into said hollow center prior to applying an isostatic load to said wire or rod.

### Claim 57 (depends on 55)

The superconducting wire or rod of claim 55, wherein said dispersant is triolein.