# US 12,480,172 B2 · Method of making a cold formable high strength steel strip and steel strip

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 12,480,172 B2
- Document ID: US12480172B2
- Status: Granted
- Kind: B2
- Application number: 17/780,451
- Filed: 2020-11-27
- Published: 2023-01-12
- Granted: 2025-11-25
- Earliest claimed: 2019-11-27
- Assignees: Tata Steel Ijmuiden B.V.
- Applicants: Tata Steel Ijmuiden B.V.
- Inventors: Radhakanta Rana
- Web page: https://patentgrep.com/patent/US12480172B2

## CPC

- C21D 8/0226: {Hot rolling}
- B32B 15/013: {one layer being formed of an iron alloy or steel, another layer being formed of a metal other than iron or aluminium}
- C21D 6/005: {containing Mn}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0236: {Cold rolling}
- C21D 8/0242: {Flattening; Dressing; Flexing}
- C21D 8/0273: {Final recrystallisation annealing}
- C21D 8/0278: involving a particular surface treatment (C21D8/0294 takes precedence)
- C21D 8/04: to produce plates or strips for drawing, e.g. for deep-drawing
- C21D 8/0426: {Hot rolling}
- C21D 8/0436: {Cold rolling}
- C21D 8/0473: {Final recrystallisation annealing}
- C21D 9/48: deep-drawing sheets
- C21D 9/52: for wires; for strips {; for rods of unlimited length}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/18: containing chromium
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/38: with more than 1.5% by weight of manganese
- C23C 2/02: Pretreatment of the material to be coated, e.g. for coating on selected surface areas (C23C2/30 takes precedence)
- C23C 2/0224: {Two or more thermal pretreatments}
- C23C 2/024: {by cleaning or etching}
- C23C 2/06: Zinc or cadmium or alloys based thereon
- C23C 2/40: Plates; Strips
- C23C 2/405: {Plates of specific length}
- C21D 2211/001: Austenite
- C21D 2211/005: Ferrite
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B32B: LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)

## Abstract

A method of manufacturing steel strip including the steps of: casting molten steel into slabs; reheating the slabs at 1150° C. or more for 1 hour or more; hot rolling the steel into a strip, preferably with an average F1 slab entry temperature above 1000° C.; coiling the hot rolled steel strip; batch annealing the steel strip: at an intercritical temperature (i.e. between Ac1 and Ac3), preferably below 700° C.; in non-oxidising and non-nitrogenated atmosphere; total annealing time at least 5 hours, preferably at least 10 hours to get Mn enrichment in austenite such that Mn content is at least 1.25 times bulk Mn content of the steel and C enrichment such that C content is at least 1.2 times bulk C content of the steel; cooling the steel after batch annealing in air, forced air or water quench.

## Claims

### Claim 1

A method of manufacturing a cold rolled and annealed steel strip, composition of the steel being in wt. %:
C: 0.05-0.3;
Mn: 3.0-12.0;
Al: 0.03-3.0;
optionally one or more further alloying elements:
Si: less than 1.5;
Cr: less than 2.0;
V: less than 0.1;
Nb: less than 0.1;
Ti: less than 0.1;
Mo: less than 0.5
inevitable impurities; and
the remainder being Fe;
the method comprising the steps of:
providinq the steel as molten steel:
casting the molten steel into a slab;
reheating the slab and holding it at a temperature of 1150° C. or more for a time of 1 hour or more;
hot rolling the steel into a hot rolled steel strip;
coiling the hot rolled steel strip;
pickling the steel strip;
intermediate-batch-annealing the coiled hot rolled steel strip at a temperature lower than 650° C. for longer than 24 hours to achieve at least 60 vol. % ferrite after cooling to room temperature;
cold rolling the intermediate-batch-annealed steel strip into a cold rolled steel strip and coiling the cold rolled steel strip to make a coiled steel strip;
batch annealing the coiled cold rolled steel strip:
at an intercritical temperature between Ac1 and Ac3 which is below 700° C.;
in a non-oxidising and non-nitrogenated atmosphere;
the total annealing time for which the steel strip is kept at said intercritical temperature being at least 5 hours in order to get Mn enrichment in austenite which is such that the Mn content is at least 1.25 times the bulk Mn content of the steel and C enrichment in austenite is such that the C content is at least 1.2 times the bulk C content of the steel;
cooling the steel strip after batch annealing in air, in forced air or by water quench.

### Claim 2 (depends on 1)

The method according to claim 1, wherein reheating the slab is at a temperature of 1200° C. or more.

### Claim 3 (depends on 1)

The method according to claim 1, wherein reheating the slab is at a temperature of 1250° C. or more.

### Claim 4 (depends on 1)

The method according to claim 1, wherein batch annealing the coiled cold rolled steel strip takes place at an intercritical temperature below 660° C.

### Claim 5 (depends on 1)

The method according to claim 1, wherein the steel strip resulting from the cooling of the steel strip after batch annealing in air, in forced air or by water quench is coated with any metallic coating applied by hot dip galvanising, galvannealing, electro-galvanising, aluminising PVD, or CVD.

### Claim 6 (depends on 1)

The method according to claim 1, wherein the steel strip resulting from the cooling of the steel strip after batch annealing in air, in forced air or by water quench steel strip undergoes skin pass rolling.

### Claim 7 (depends on 6)

The method according to claim 6, wherein the skin pass rolling takes place with a thickness reduction of 5% or less.

### Claim 8 (depends on 1)

The method according to claim 1,
wherein the batch annealed steel strip has the Mn enrichment in austenite which is such that the Mn content is at least 1.4 times the bulk Mn content of the steel and the C enrichment in austenite is such that the C content is at least 2.3 times the bulk C content of the steel, in order to obtain metastable retained austenite to give the steel after batch annealing a high strain hardening exponent of at least 0.3 measured after yield point elongation for a strain range of 7% in a quasi-static tensile test,
wherein the steel after batch annealing has a microstructure that comprises in vol.
ferrite: 30-70%;
retained austenite: 20-65%;
martensite: <20%, including 0 vol. %.

### Claim 9 (depends on 8)

The method according to claim 8, wherein a length/width ratio of grains of the ferrite is 3 or smaller.

### Claim 10 (depends on 8)

The method according to claim 8, wherein the steel strip resulting from the cooling of the steel strip after batch annealing in air, in forced air or by water quench has a yield point elongation of a maximum of 10% engineering strain measured from its engineering stress-strain curve.

### Claim 11 (depends on 8)

The method according to claim 8, wherein the steel strip resulting from the cooling of the steel strip after batch annealing in air, in forced air or by water quench has a yield strength of 600 MPa or more and an ultimate tensile strength of 800 MPa or more and a total elongation (A80) of 20% or more.

### Claim 12 (depends on 8)

The method according to claim 8, wherein the steel strip resulting from the cooling of the steel strip after batch annealing in air, in forced air or by water quench has a very high formability characterized by an individual direction stretching strain in biaxial stretching condition of 10% or more, a VDA bending angle at 1.0 mm thickness of 100° or more and a hole expansion capacity of 20% or more.

### Claim 13 (depends on 1)

The method according to claim 1, wherein the inevitable impurities have
S: less than 20 ppm;
P: less than 0.04.

### Claim 14 (depends on 5)

The method according to claim 5, wherein the resulting strip is coated with any metallic coating applied by hot dip galvanising, galvannealing, electro-galvanising, or aluminising.

### Claim 15 (depends on 5)

The method according to claim 5, wherein the resulting strip is coated with any metallic coating applied by PVD or CVD.

### Claim 16 (depends on 1)

The method according to claim 1, wherein the hot rolling of the steel into the hot rolled steel strip has an average F1 slab entry temperature of above 1000° C.

### Claim 17 (depends on 1)

The method according to claim 1, wherein the total annealing time for which the steel strip is kept at said intercritical temperature being at least 10 hours.