# US 11,118,254 B2 · Thermal treatment method for aluminum alloy cast-spun wheel

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 11,118,254 B2
- Document ID: US11118254B2
- Status: Granted
- Kind: B2
- Application number: 16/127,581
- Filed: 2018-09-11
- Published: 2019-03-14
- Granted: 2021-09-14
- Earliest claimed: 2017-09-13
- Assignees: CITIC Dicastal Co., Ltd.
- Applicants: CITIC Dicastal CO., LTD.
- Inventors: Zuo Xu; Guoyuan Xiong; Honglei Liu; Hongfeng Liu; Rui Wang; Changhai Li
- Web page: https://patentgrep.com/patent/US11118254B2

## CPC

- C22F 1/04: of aluminium or alloys based thereon
- C22F 1/002: {by rapid cooling or quenching; cooling agents used therefor}
- C22F: CHANGING THE PHYSICAL STRUCTURE OF NON-FERROUS METALS AND NON-FERROUS ALLOYS (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass, C23F17/00)

## Abstract

A thermal treatment method for an A356 aluminum alloy cast-spun wheel is provided. The thermal treatment method is characterized by including the steps of: 1) heating an aluminum alloy wheel cast-spun piece to 540-550° C.; 2) preserving the heat of the aluminum alloy wheel cast-spun piece for 275-285 minutes at the temperature of 540-550° C.; 3) quenching the aluminum alloy wheel cast-spun piece in water of 70-90° C. for 180 seconds; 4) heating the aluminum alloy wheel cast-spun piece to 150-160° C.; 5) preserving the heat of the aluminum alloy wheel cast-spun piece for 175-185 minutes at 150-160° C.; and 6) cooling the aluminum alloy wheel cast-spun piece in air to room temperature.

## Claims

### Claim 1

A thermal treatment method for an aluminum alloy wheel produced by casting and spinning, comprising the steps of:
1) heating the aluminum alloy wheel produced by casting and spinning to 540-550° C.;
2) preserving the heat of the aluminum alloy wheel produced by casting and spinning for 275-285 minutes 540-550° C.;
3) quenching the aluminum alloy wheel produced by casting and spinning in 70-90° C. water for 180 seconds;
4) heating the aluminum alloy wheel produced by casting and spinning to 150-160° C.;
5) preserving the heat of the aluminum alloy wheel produced by casting and spinning for 175-185 minutes at 150-160° C.; and
6) cooling the aluminum alloy wheel produced by casting and spinning in air to room temperature.

### Claim 2 (depends on 1)

The thermal treatment method for the aluminum alloy wheel produced by casting and spinning according to claim 1, wherein uniform heating is ensured in step 1).

### Claim 3 (depends on 1)

The method according to claim 1, wherein a time for transferring the aluminum alloy wheel produced by casting and spinning from a heat preservation state to a quenching tank in step 3) is within 20 seconds.

### Claim 4 (depends on 1)

The thermal treatment method for the aluminum alloy wheel produced by casting and spinning according to claim 1, wherein uniform heating is ensured in step 4).

### Claim 5 (depends on 1)

The thermal treatment method for the aluminum alloy wheel produced by casting and spinning according to claim 1, wherein before step 5), the thermal treatment method for the aluminum alloy wheel produced by casting and spinning further comprises a step of performing short-time thermal shock on the aluminum alloy wheel produced by casting and spinning, wherein a time for the short-time thermal shock is 1-3 minutes, and a temperature for the short-time thermal shock is 540-550° C.

### Claim 6 (depends on 1)

The thermal treatment method for the aluminum alloy wheel produced by casting and spinning according to claim 1, wherein a quenching medium is agitated in step 3).