# US 11,118,240 B2 · Abrasion-resistant steel plate and method of producing abrasion-resistant steel plate

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 11,118,240 B2
- Document ID: US11118240B2
- Status: Granted
- Kind: B2
- Application number: 16/092,538
- Filed: 2016-04-19
- Published: 2019-04-25
- Granted: 2021-09-14
- Earliest claimed: 2016-04-19
- Assignees: Jfe Steel Corporation
- Applicants: Jfe Steel Corporation
- Inventors: Yusuke Terazawa; Naoki Takayama; Kenji Hayashi; Kazukuni Hase
- Web page: https://patentgrep.com/patent/US11118240B2

## CPC

- C21D 8/0263: {following hot rolling}
- B22D 11/001: {of specific alloys}
- B22D 11/1206: {for plastic shaping of strands (rolling mills B21B1/46)}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/0226: {Hot rolling}
- C21D 9/46: for sheet metals
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/005: {containing rare earths, i.e. Sc, Y, Lanthanides}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/18: containing chromium
- C22C 38/20: with copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/24: with vanadium
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/32: with boron
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/40: with nickel
- C22C 38/50: with titanium or zirconium
- C22C 38/54: with boron
- C21D 2211/004: Dispersions; Precipitations
- C21D 2211/008: Martensite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B22D: CASTING OF METALS; CASTING OF OTHER SUBSTANCES BY THE SAME PROCESSES OR DEVICES (shaping of plastics or substances in a plastic state B29C; metallurgical processing, selection of substances to be added to metal C21, C22)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

An abrasion-resistant steel plate comprises: a chemical composition containing, in mass %, C: 0.20% to 0.45%, Si: 0.01% to 1.0%, Mn: 0.3% to 2.5%, P: 0.020% or less, S: 0.01% or less, Cr: 0.01% to 2.0%, Ti: 0.10% to 1.00%, B: 0.0001% to 0.0100%, Al: 0.1% or less, N: 0.01% or less, and a balance consisting of Fe and inevitable impurities; and a microstructure in which a volume fraction of martensite is 90% or more, and a prior austenite grain size is 80 μm or less, wherein a number density of TiC precipitate having a size of 0.5 μm or more is 400 particles/mm2 or more, and a Mn content [Mn] and a P content [P] in a plate thickness central segregation area satisfy 0.04[Mn]+[P]<0.50.

## Claims

### Claim 1

An abrasion-resistant steel plate comprising:
a chemical composition containing, in mass %,
C: 0.20% to 0.45%,
Si: 0.01% to 1.0%,
Mn: 0.3% to 2.5%,
P: 0.020% or less,
S: 0.01% or less,
Cr: 0.01% to 2.0%,
Ti: 0.10% to 1.00%,
B: 0.0001% to 0.0100%,
Al: 0.1% or less,
N: 0.01% or less, and
a balance consisting of Fe and inevitable impurities; and
a microstructure in which a volume fraction of martensite at a depth of 1 mm from a surface of the abrasion-resistant steel plate is 90% or more, and a prior austenite grain size at the mid-thickness of the abrasion-resistant steel plate is 80 μm or less,
wherein a number density of TiC precipitates having a size of 0.5 μm or more at a depth of 1 mm from the surface of the abrasion-resistant steel plate is 400 particles/mm2 or more, and
a concentration [Mn] of Mn in mass % and a concentration [P] of P in mass % in a plate thickness central segregation area satisfy the following Expression (1):
0.04[Mn]+[P]<0.50 (1).

### Claim 2 (depends on 1)

The abrasion-resistant steel plate according to claim 1,
wherein the chemical composition further contains, in mass %, one or more elements selected from the group consisting of
Cu: 0.01% to 2.0%,
Ni: 0.01% to 10.0%,
Mo: 0.01% to 3.0%,
Nb: 0.001% to 0.100%,
V: 0.001% to 1.00%,
W: 0.01% to 1.5%,
Ca: 0.0001% to 0.0200%,
Mg: 0.0001% to 0.0200%, and
REM: 0.0005% to 0.0500%.

### Claim 3 (depends on 1)

The abrasion-resistant steel plate according to claim 1,
wherein a reduction of area in a tensile test of the abrasion-resistant steel plate after subjecting the abrasion-resistant steel plate to temper embrittlement treatment and subsequent hydrogen embrittlement treatment is 10% or more.

### Claim 4 (depends on 2)

The abrasion-resistant steel plate according to claim 2,
wherein a reduction of area in a tensile test of the abrasion-resistant steel plate after subjecting the abrasion-resistant steel plate to temper embrittlement treatment and subsequent hydrogen embrittlement treatment is 10% or more.

### Claim 5 (depends on 1)

A method of producing the abrasion-resistant steel plate according to claim 1, the method comprising:
subjecting molten steel to continuous casting, to form a slab;
heating the slab to 1000° C. to 1300° C.;
subjecting the heated slab to hot rolling in which reduction rolling with a rolling shape factor of 0.7 or more and a rolling reduction of 7% or more at a plate thickness central part temperature of 950° C. or more is performed three times or more, to obtain a hot-rolled steel plate;
reheating the hot-rolled steel plate to a reheating quenching temperature; and
quenching the reheated hot-rolled steel plate,
wherein the slab has the chemical composition according to claim 1,
in the continuous casting, light reduction rolling with a rolling reduction gradient of 0.4 mm/m or more is performed twice or more, upstream from a final solidification position of the slab,
the reheating quenching temperature is Ac3 to 1050° C., and
an average cooling rate from 650° C. to 300° C. in the quenching is 1° C./s or more.

### Claim 6 (depends on 2)

A method of producing the abrasion-resistant steel plate according to claim 2, the method comprising:
subjecting molten steel to continuous casting, to form a slab;
heating the slab to 1000° C. to 1300° C.;
subjecting the heated slab to hot rolling in which reduction rolling with a rolling shape factor of 0.7 or more and a rolling reduction of 7% or more at a plate thickness central part temperature of 950° C. or more is performed three times or more, to obtain a hot-rolled steel plate;
reheating the hot-rolled steel plate to a reheating quenching temperature; and
quenching the reheated hot-rolled steel plate,
wherein the slab has the chemical composition according to claim 2,
in the continuous casting, light reduction rolling with a rolling reduction gradient of 0.4 mm/m or more is performed twice or more, upstream from a final solidification position of the slab,
the reheating quenching temperature is Ac3 to 1050° C., and
an average cooling rate from 650° C. to 300° C. in the quenching is 1° C./s or more.

### Claim 7 (depends on 5)

The method according to claim 5, further comprising
tempering the quenched hot-rolled steel plate at a tempering temperature of 100° C. to 300° C.

### Claim 8 (depends on 6)

The method according to claim 6, further comprising
tempering the quenched hot-rolled steel plate at a tempering temperature of 100° C. to 300° C.

### Claim 9 (depends on 1)

A method of producing the abrasion-resistant steel plate according to claim 1, the method comprising:
subjecting molten steel to continuous casting, to form a slab;
heating the slab to 1000° C. to 1300° C.;
subjecting the heated slab to hot rolling in which reduction rolling with a rolling shape factor of 0.7 or more and a rolling reduction of 7% or more at a plate thickness central part temperature of 950° C. or more is performed three times or more, to obtain a hot-rolled steel plate; and
direct quenching the hot-rolled steel plate,
wherein the slab has the chemical composition according to claim 1,
in the continuous casting, light reduction rolling with a rolling reduction gradient of 0.4 mm/m or more is performed twice or more, upstream from a final solidification position of the slab,
a direct quenching temperature in the direct quenching is Ac3 or more, and
an average cooling rate from 650° C. to 300° C. in the direct quenching is 1° C./s or more.

### Claim 10 (depends on 2)

A method of producing the abrasion-resistant steel plate according to claim 2, the method comprising:
subjecting molten steel to continuous casting, to form a slab;
heating the slab to 1000° C. to 1300° C.;
subjecting the heated slab to hot rolling in which reduction rolling with a rolling shape factor of 0.7 or more and a rolling reduction of 7% or more at a plate thickness central part temperature of 950° C. or more is performed three times or more, to obtain a hot-rolled steel plate; and
direct quenching the hot-rolled steel plate,
wherein the slab has the chemical composition according to claim 2,
in the continuous casting, light reduction rolling with a rolling reduction gradient of 0.4 mm/m or more is performed twice or more, upstream from a final solidification position of the slab,
a direct quenching temperature in the direct quenching is Ac3 or more, and
an average cooling rate from 650° C. to 300° C. in the direct quenching is 1° C./s or more.

### Claim 11 (depends on 9)

The method according to claim 9, further comprising
tempering the quenched hot-rolled steel plate at a tempering temperature of 100° C. to 300° C.

### Claim 12 (depends on 10)

The method according to claim 10, further comprising
tempering the quenched hot-rolled steel plate at a tempering temperature of 100° C. to 300° C.

### Claim 13 (depends on 1)

The abrasion-resistant steel plate according to claim 1,
wherein the prior austenite grain size at the mid-thickness of the abrasion-resistant steel plate is 11 μm or more and 80 μm or less.