# US 11,117,120 B2 · Catalyst for synthesizing carbon nanotube and method of synthesizing carbon nanotube

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 11,117,120 B2
- Document ID: US11117120B2
- Status: Granted
- Kind: B2
- Application number: 16/174,456
- Filed: 2018-10-30
- Published: 2019-05-02
- Granted: 2021-09-14
- Earliest claimed: 2017-10-31
- Assignees: SK Innovation Co., Ltd.; SK Global Chemical Co., Ltd.
- Applicants: SK Innovation Co., Ltd.; SK Global Chemical Co., Ltd.
- Inventors: Hye Ryun Seo; Yong Tak Kwon
- Web page: https://patentgrep.com/patent/US11117120B2

## CPC

- B01J 21/04: Alumina
- B01J 23/8892: {Manganese}
- B01J 21/02: Boron or aluminium; Oxides or hydroxides thereof
- B01J 21/185: {Carbon nanotubes (carbon nanotubes per se C01B32/15)}
- B01J 37/0201: {Impregnation}
- B01J 37/04: Mixing {(B01J37/0009, B01J37/0018 take precedence)}
- B01J 37/08: Heat treatment {(B01J37/0009, B01J37/0018 take precedence)}
- C01B 32/162: characterised by catalysts
- B01J 2523/00: Constitutive chemical elements of heterogeneous catalysts
- B01J 2523/31: Aluminium
- B01J 2523/72: Manganese
- B01J 2523/845: Cobalt
- B01J: CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
- C01B: NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; {METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C}

## Abstract

A catalyst for synthesizing a carbon nanotube includes a support containing a metal, and an active metal impregnated on the support. The active metal includes cobalt and manganese. A surface molar ratio of the active metal relative to the metal of the support is 40% or less of a bulk molar ratio of the active metal relative to the metal of the support. A carbon nanotube having high purity and low resistance is obtained from the catalyst.

## Claims

### Claim 1

A catalyst for synthesizing a carbon nanotube, including:
a support containing a metal, the metal including aluminum; and
an active metal impregnated on the support, the active metal including cobalt and manganese,
wherein a surface molar ratio of the active metal relative to the metal of the support is 40% or less of a bulk molar ratio of the active metal relative to the metal of the support, wherein the surface molar ratio is an average molar ratio of the active metal measured within a thickness of 10 nm from an outermost surface of the catalyst, and the bulk molar ratio is an average molar ratio of the active metal throughout the catalyst, and
wherein the surface molar ratio of the active metal is in a range from 0.03 to 0.06 relative to aluminum in the support, and the bulk molar ratio of the active metal is in a range from 0.15 to 0.29 relative to aluminum in the support.

### Claim 2 (depends on 1)

The catalyst according to claim 1, wherein the surface molar ratio of the active metal is in a range from 10% to 30% of the bulk molar ratio of the active metal.

### Claim 3 (depends on 1)

The catalyst according to claim 1, wherein the surface molar ratio is represented by Equation 1 below:
aluminum (Al): cobalt (Co): manganese (Mn)=1:x1:y1 [Equation 1]
wherein in Equation 1, 0.02≤x1≤0.04, 0.01≤y1≤0.02.

### Claim 4 (depends on 3)

The catalyst according to claim 3, wherein, in Equation 1, 0.0200≤x1≤0.0375, 0.0130≤y1≤0.0189.

### Claim 5 (depends on 1)

The catalyst according to claim 1, wherein the bulk molar ratio is represented by Equation 2 below:
aluminum (Al): cobalt (Co): manganese (Mn)=1:x2:y2 [Equation 2]
wherein in Equation 2, 0.08≤x2≤0.15, 0.07≤y2≤0.14.

### Claim 6 (depends on 1)

The catalyst according to claim 1, wherein the active metal consists of cobalt and manganese.

### Claim 7 (depends on 1)

A method of synthesizing a carbon nanotube, comprising:
preparing a support containing a metal, a cobalt precursor and a manganese precursor;
mixing the support, the cobalt precursor and the manganese precursor with changing molar ratios to form a catalyst knead;
performing a thermal treatment on the catalyst knead to form the catalyst of claim 1 for synthesizing a carbon nanotube; and
forming a carbon nanotube using the catalyst.

### Claim 8 (depends on 7)

The method according to claim 7, wherein, in the formation of the catalyst knead, the cobalt precursor and the manganese precursor are mixed so that a surface molar ratio of cobalt and manganese relative to the metal in the support is less than a bulk molar ratio of cobalt and manganese relative to the metal in the support.

### Claim 9 (depends on 8)

The method according to claim 8, wherein the support includes an aluminum oxide, and
the surface molar ratio and the bulk molar ratio of the catalyst are represented by Equation 1 and Equation 2, respectively:
aluminum (Al): cobalt (Co): manganese (Mn)=1:x1:y1 [Equation 1]
wherein in Equation 1, 0.02≤x1≤0.04, 0.01≤y1≤0.02,
aluminum (Al): cobalt (Co): manganese (Mn)=1:x2:y2 [Equation 2]
wherein in Equation 2, 0.08≤x2≤0.15, 0.07≤y2≤0.14.

### Claim 10 (depends on 7)

The method according to claim 7, wherein performing the thermal treatment includes:
drying the catalyst knead at a temperature in a range from 100° C. to 150° C.; and
calcinating the dried catalyst knead at a temperature in a ranging from 400° C. to 600° C.

### Claim 11 (depends on 7)

The method according to claim 7, wherein forming the carbon nanotube includes a chemical vapor deposition or a chemical vapor synthesis.

### Claim 12 (depends on 7)

The method according to claim 7, wherein the cobalt precursor includes cobalt nitrate or a hydrate thereof, and the manganese precursor includes manganese nitrate or a hydrate thereof.