# US 10,954,576 B2 · High-strength steel, method for manufacturing high-strength steel, steel pipe, and method for manufacturing steel pipe

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 10,954,576 B2
- Document ID: US10954576B2
- Status: Granted
- Kind: B2
- Application number: 15/560,013
- Filed: 2015-03-27
- Published: 2018-03-08
- Granted: 2021-03-23
- Earliest claimed: 2015-03-27
- Assignees: Jfe Steel Corporation
- Applicants: Jfe Steel Corporation
- Inventors: Shusaku Ota; Junji Shimamura; Nobuyuki Ishikawa; Shigeru Endo
- Web page: https://patentgrep.com/patent/US10954576B2

## CPC

- C21D 9/08: for tubular bodies or pipes
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/02: during manufacturing of plates or strips (C21D8/12 takes precedence)
- C21D 8/10: during manufacturing of tubular bodies
- C21D 9/46: for sheet metals
- C22C 38/00: Ferrous alloys, e.g. steel alloys (cast-iron alloys C22C37/00)
- C22C 38/001: {containing N}
- C22C 38/002: {containing In, Mg, or other elements not provided for in one single group C22C38/001 - C22C38/60}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/06: containing aluminium
- C22C 38/08: containing nickel {(C22C38/105 takes precedence)}
- C22C 38/12: containing tungsten, tantalum, molybdenum, vanadium, or niobium
- C22C 38/14: containing titanium or zirconium
- C22C 38/16: containing copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/26: with niobium or tantalum
- C22C 38/28: with titanium or zirconium
- C22C 38/38: with more than 1.5% by weight of manganese
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/46: with vanadium
- C22C 38/48: with niobium or tantalum
- C22C 38/50: with titanium or zirconium
- C22C 38/58: with more than 1.5% by weight of manganese
- C21D 2211/002: Bainite
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- C22C: ALLOYS (treatment of alloys C21D, C22F)

## Abstract

A high-strength steel having a specified chemical composition, wherein parameter Peff is 0.050% or more, the relationship (TS0−TS)/TS0≤0.050 is satisfied, wherein TS is defined as tensile strength determined at a temperature of 350° C. after aging has been performed under the condition of a Larson-Miller Parameter (LMP) of 15700, and wherein TS0 is defined as tensile strength determined at a temperature of 350° C. before the aging is performed, and having a toughness represented by a vE−20 of 100 J or more in a weld heat-affected zone, which is formed when welding is performed.

## Claims

### Claim 1

A high-strength steel
having a chemical composition containing, by mass %, C: 0.040% to 0.090%, Si: 0.05% to 0.30%, Mn: 1.50% to 2.50%, P: 0.020% or less, S: 0.002% or less, Mo: 0.20% to 0.60%, Nb: 0.020% to 0.070%, Ti: 0.020% or less, V: 0.080% or less, Al: 0.045% or less, N: 0.0100% or less, and the balance being Fe and inevitable impurities, wherein the high-strength steel:
has a parameter Peff, as calculated by equation (1):
Peff(%)=(0.13Nb+0.24V−0.125Ti)/(C+0.86N) (1),
is of 0.070% or more, wherein the symbols of the chemical elements in equation (1) respectively denote the contents (mass %) of the corresponding chemical elements, and wherein the symbol of a chemical element which is not included is assigned a value of 0;
satisfies the relationship (TS0−TS)/TS0≤0.050, wherein TS is defined as tensile strength determined at a temperature of 350° C. after aging has been performed under the condition of a Larson-Miller Parameter (LMP) of 15700, and wherein TS0 is defined as tensile strength determined at a temperature of 350° C. before the aging is performed,
wherein the high-strength steel has a yield strength of 555 MPa or more and the tensile strengths of 620 MPa or more determined at a temperature of 350° C., both before and after aging has been performed under the condition of the LMP, and
wherein the high-strength steel has a microstructure comprising a bainite phase fraction of 70% or more in terms of area fraction.

### Claim 2 (depends on 1)

The high-strength steel according to claim 1, wherein a value of Ti/N is in the range of 2.0 to 4.0, and X, as calculated by equation (2):
X=0.35Cr+0.9Mo+12Nb+8V (2),
is 0.70% or more, wherein the symbols of the chemical elements in equation (2) respectively denote the contents (mass %) of the corresponding chemical elements, and wherein the symbol of a chemical element which is not included is assigned a value of 0.

### Claim 3 (depends on 1)

The high-strength steel according to claim 1, the chemical composition of the high-strength steel further contains, by mass %, one, two, or more of:
Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, and Ca: 0.0005% to 0.0040%.

### Claim 4 (depends on 1)

A steel pipe composed of the high-strength steel according to claim 1, wherein butt portions of a steel plate are welded to form a pipe shape and wherein a weld heat-affected zone formed during welding has a toughness represented by a vE−20 of 100 J or more.

### Claim 5 (depends on 1)

A method for manufacturing the high-strength steel according to claim 1, the method comprising:
a heating process wherein a steel raw material is heated to a temperature of 1050° C. to 1200° C.;
a hot rolling process wherein the steel raw material, which has been heated in the heating process, is hot-rolled under the conditions of an accumulated rolling reduction ratio in a temperature range of 900° C. or lower of 50% or more and a rolling finish temperature of 850° C. or lower;
an accelerated cooling process wherein the hot-rolled steel plate, which has been obtained in the hot rolling process, is subjected to accelerated cooling under the conditions of a cooling rate of 5° C./s or more and a cooling stop temperature of 250° C. to 550° C.; and
a reheating process wherein the hot-rolled steel plate is reheated, immediately after the accelerated cooling has been finished, under the conditions of a heating rate of 0.5° C./s or more and an end-point temperature of 550° C. to 700° C.

### Claim 6 (depends on 1)

A method for manufacturing a steel pipe, the method comprising:
a cold forming process wherein a steel plate composed of the high-strength steel according to claim 1 is subjected to cold forming so as to be formed into a pipe shape; and
a welding process wherein butt portions of the steel plate, which has been formed into a pipe shape in the cold forming process, are welded.

### Claim 7 (depends on 2)

The high-strength steel according to claim 2, the chemical composition of the high-strength steel further contains, by mass %, one, two, or more of:
Cu: 0.50% or less, Ni: 0.50% or less, Cr: 0.50% or less, and Ca: 0.0005% to 0.0040%.

### Claim 8 (depends on 2)

A steel pipe composed of the high-strength steel according to claim 2, wherein butt portions of a steel plate are welded to form a pipe shape and wherein a weld heat-affected zone formed during welding has a toughness represented by a vE−20 of 100 J or more.

### Claim 9 (depends on 3)

A steel pipe composed of the high-strength steel according to claim 3, wherein butt portions of a steel plate are welded to form a pipe shape and wherein a weld heat-affected zone formed during welding has a toughness represented by a vE−20 of 100 J or more.

### Claim 10 (depends on 7)

A steel pipe composed of the high-strength steel according to claim 7, wherein butt portions of a steel plate are welded to form a pipe shape and wherein a weld heat-affected zone formed during welding has a toughness represented by a VE−20 of 100 J or more.

### Claim 11 (depends on 2)

A method for manufacturing the high-strength steel according to claim 2, the method comprising:
a heating process wherein a steel raw material is heated to a temperature of 1050° C. to 1200° C.;
a hot rolling process wherein the steel raw material, which has been heated in the heating process, is hot-rolled under the conditions of an accumulated rolling reduction ratio in a temperature range of 900° C. or lower of 50% or more and a rolling finish temperature of 850° C. or lower;
an accelerated cooling process wherein the hot-rolled steel plate, which has been obtained in the hot rolling process, is subjected to accelerated cooling under the conditions of a cooling rate of 5° C./s or more and a cooling stop temperature of 250° C. to 550° C.; and
a reheating process wherein the hot-rolled steel plate is reheated, immediately after the accelerated cooling has been finished, under the conditions of a heating rate of 0.5° C./s or more and an end-point temperature of 550° C. to 700° C.

### Claim 12 (depends on 3)

A method for manufacturing the high-strength steel according to claim 3, the method comprising:
a heating process wherein a steel raw material is heated to a temperature of 1050° C. to 1200° C.;
a hot rolling process wherein the steel raw material, which has been heated in the heating process, is hot-rolled under the conditions of an accumulated rolling reduction ratio in a temperature range of 900° C. or lower of 50% or more and a rolling finish temperature of 850° C. or lower;
an accelerated cooling process wherein the hot-rolled steel plate, which has been obtained in the hot rolling process, is subjected to accelerated cooling under the conditions of a cooling rate of 5° C./s or more and a cooling stop temperature of 250° C. to 550° C.; and
a reheating process wherein the hot-rolled steel plate is reheated, immediately after the accelerated cooling has been finished, under the conditions of a heating rate of 0.5° C./s or more and an end-point temperature of 550° C. to 700° C.

### Claim 13 (depends on 7)

A method for manufacturing the high-strength steel according to claim 7, the method comprising:
a heating process wherein a steel raw material is heated to a temperature of 1050° C. to 1200° C.;
a hot rolling process wherein the steel raw material, which has been heated in the heating process, is hot-rolled under the conditions of an accumulated rolling reduction ratio in a temperature range of 900° C. or lower of 50% or more and a rolling finish temperature of 850° C. or lower;
an accelerated cooling process wherein the hot-rolled steel plate, which has been obtained in the hot rolling process, is subjected to accelerated cooling under the conditions of a cooling rate of 5° C./s or more and a cooling stop temperature of 250° C. to 550° C.; and
a reheating process wherein the hot-rolled steel plate is reheated, immediately after the accelerated cooling has been finished, under the conditions of a heating rate of 0.5° C./s or more and an end-point temperature of 550° C. to 700° C.

### Claim 14 (depends on 2)

A method for manufacturing a steel pipe, the method comprising:
a cold forming process wherein a steel plate composed of the high-strength steel according to claim 2 is subjected to cold forming so as to be formed into a pipe shape; and
a welding process wherein butt portions of the steel plate, which has been formed into a pipe shape in the cold forming process, are welded.

### Claim 15 (depends on 3)

A method for manufacturing a steel pipe, the method comprising:
a cold forming process wherein a steel plate composed of the high-strength steel according to claim 3 is subjected to cold forming so as to be formed into a pipe shape; and
a welding process wherein butt portions of the steel plate, which has been formed into a pipe shape in the cold forming process, are welded.

### Claim 16 (depends on 7)

A method for manufacturing a steel pipe, the method comprising:
a cold forming process wherein a steel plate composed of the high-strength steel according to claim 7 is subjected to cold forming so as to be formed into a pipe shape; and
a welding process wherein butt portions of the steel plate, which has been formed into a pipe shape in the cold forming process, are welded.