# US 10,954,136 B2 · Preparation method and application of tetragonal NaV2O5⋅H2O nanosheet-like powder

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 10,954,136 B2
- Document ID: US10954136B2
- Status: Granted
- Kind: B2
- Application number: 16/202,002
- Filed: 2018-11-27
- Published: 2019-05-09
- Granted: 2021-03-23
- Earliest claimed: 2018-02-06
- Assignees: Shaanxi University of Science and Technology
- Applicants: Shaanxi University of Science and Technology
- Inventors: Jianfeng Huang; Wenbin Li; Liyun Cao; Liangliang Feng; Shuwei He; Yijie Ren; Ruizi Li; Xunwei Chang
- Web page: https://patentgrep.com/patent/US10954136B2

## CPC

- C01G 31/02: Oxides
- C01G 31/00: Compounds of vanadium
- H01M 4/485: of mixed oxides or hydroxides for inserting or intercalating light metals, e.g. LiTi2O4 or LiTi2OxFy (H01M4/505, H01M4/525 take precedence)
- C01P 2002/72: by d-values or two theta-values, e.g. as X-ray diagram
- C01P 2004/03: obtained by SEM
- C01P 2004/04: obtained by TEM, STEM, STM or AFM
- C01P 2004/24: Nanoplates, i.e. plate-like particles with a thickness from 1-100 nanometer
- C01P 2004/30: extending in three dimensions
- C01P 2006/40: Electric properties
- H01M 4/5825: {Oxygenated metallic salts or polyanionic structures, e.g. borates, phosphates, silicates, olivines}
- H01M 10/0525: Rocking-chair batteries, i.e. batteries with lithium insertion or intercalation in both electrodes; Lithium-ion batteries
- H01M 2004/027: {Negative electrodes}
- Y02E 60/10: Energy storage using batteries
- C01G: COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F (metal hydrides {monoborane, diborane or addition complexes thereof} C01B6/00; salts of oxyacids of halogens C01B11/00; peroxides, salts or peroxyacids C01B15/00; thiosulfates, dithionites, polythionates C01B17/64; compounds containing selenium, or tellurium C01B19/00; binary compounds of nitrogen with metals C01B21/06; azides C01B21/08; {compounds containing nitrogen, other non-metals and metal C01B21/082}; metal amides C01B21/092; nitrites C01B21/50; {compounds of noble gases C01B23/0005}; phosphides C01B25/08; salts of oxyacids of phosphorus C01B25/16; carbides C01B32/90; compounds containing silicon C01B33/00; compounds containing boron C01B35/00; compounds having molecular sieve properties but not having base-exchange properties C01B37/00; compounds having molecular sieve and base-exchange properties, e.g. crystalline zeolites, C01B39/00; cyanides C01C3/08; salts of cyanamide C01C3/16; thiocyanates C01C3/20)
- H01M: PROCESSES OR MEANS, e.g. BATTERIES, FOR THE DIRECT CONVERSION OF CHEMICAL ENERGY INTO ELECTRICAL ENERGY
- C01P: INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- Y02E: REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION

## Abstract

A preparation method of a tetragonal NaV2O5.H2O nanosheet-like powder includes steps of: (S1) simultaneously adding NaVO3 and Na2S.9H2O into deionized water, and then magnetically stirring, and obtaining a black turbid solution; (S2) sealing after putting the black turbid solution into an inner lining of a reaction kettle, fixing the sealed inner lining in an outer lining of the reaction kettle, placing the reaction kettle into a homogeneous reactor, and then performing a hydrothermal reaction; and (S3) after completing the hydrothermal reaction, naturally cooling the reaction kettle to the room temperature, and then alternately cleaning through water and alcohol, and then collecting a product, drying the product, and finally obtaining the tetragonal NaV2O5.H2O nanosheet-like powder with a thickness in a range of 30-60 nm and a single crystal structure grown along a (002) crystal orientation.

## Claims

### Claim 1

A tetragonal NaV2O5.H2O nanosheet-like powder used as an anode material of a lithium ion battery and prepared by a preparation method which comprises steps of:
(S1) simultaneously adding 0.8-1.2 g of NaVO3 and 0.5-3.5 g of Na2S.9H2O into 55-65 ml of deionized water, and then magnetically stirring for 55-65 min under a rotational speed in a range of 800-1000 r/min, and obtaining a black turbid solution;
(S2) sealing after putting the black turbid solution into an inner lining of a reaction kettle according to a filling ratio in a range of 55-65%, fixing the sealed inner lining in an outer lining of the reaction kettle, placing the reaction kettle into a homogeneous reactor, and then heating under a rotational speed in a range of 5-15 r/min from a room temperature to 150-200° C., and then performing a hydrothermal reaction for 1-36 h; and
(S3) after completing the hydrothermal reaction, naturally cooling, the reaction kettle to the room temperature, and then alternately cleaning with water and alcohol by suction filtration or centrifugation for 3-6 times, and then collecting a product by suction filtration or centrifugation, drying the product at 40-80° C., and finally obtaining the tetragonal NaV2O5.H2O nanosheet-like powder, wherein:
the tetragonal NaV2O5.H2O nanosheet-like powder has a thickness in a range of 30-60 nm, a layer spacing of 7.71 Å, and is a single crystal layered structure grown along a (002) crystal orientation;
when the tetragonal NaV2O5.H2O nanosheet-like powder acts as the anode material of the lithium ion battery, at a current density of 100, 200, 500, 1000 and 2000 mAg−1, a capacity reaches 348, 285, 209, 167 and 130 mAhg−1, respectively; at the current density of 100 and 200 mAg−1, a first discharge capacity reaches 859 and 633 mAhg−1, respectively; and after 480 and 600 cycles, the capacity reaches 483 and 320 mAhg−1, respectively; and after 1000 cycles at the current density of 1000 mAg−1, the capacity reaches 129 mAhg−1.