# US 10,953,465 B2 · 3D printable hard ferrous metallic alloys for powder bed fusion

> Agents: this data is available as JSON from the patentgrep API and MCP server — see https://patentgrep.com/llms.txt

- Number: US 10,953,465 B2
- Document ID: US10953465B2
- Status: Granted
- Kind: B2
- Application number: 16/393,194
- Filed: 2019-04-24
- Published: 2019-08-29
- Granted: 2021-03-23
- Earliest claimed: 2016-11-01
- Assignees: The NanoSteel Company, Inc.
- Applicants: Formetrix, Inc.
- Inventors: Charles D. Tuffile; Harald Lemke
- Web page: https://patentgrep.com/patent/US10953465B2

## CPC

- C21D 1/18: Hardening (C21D1/02 takes precedence); Quenching with or without subsequent tempering (quenching devices C21D1/62)
- B22F 10/00: Additive manufacturing of workpieces or articles from metallic powder (apparatus or devices therefor B22F12/00)
- B22F 10/20: Direct sintering or melting
- B22F 10/28: Powder bed fusion, e.g. selective laser melting [SLM] or electron beam melting [EBM]
- B22F 10/32: of the atmosphere, e.g. composition or pressure in a building chamber
- B22F 10/36: of energy beam parameters
- B22F 12/17: to heat the build chamber or platform
- B23K 15/0086: {welding for purposes other than joining, e.g. build-up welding}
- B23K 26/0006: {taking account of the properties of the material involved (B23K26/32, B23K26/40 take precedence)}
- B23K 26/342: Build-up welding
- B33Y 10/00: Processes of additive manufacturing
- B33Y 40/00: Auxiliary operations or equipment, e.g. for material handling
- B33Y 70/00: Materials specially adapted for additive manufacturing
- C21D 1/613: Gases; Liquefied or solidified normally gaseous material
- C21D 6/002: {containing Cr (C21D6/004 takes precedence)}
- C21D 6/004: {containing Cr and Ni}
- C21D 6/005: {containing Mn}
- C21D 6/008: {containing Si}
- C21D 8/0257: {with diffusion of elements, e.g. decarburising, nitriding}
- C22C 38/001: {containing N}
- C22C 38/02: containing silicon
- C22C 38/04: containing manganese
- C22C 38/20: with copper
- C22C 38/22: with molybdenum or tungsten
- C22C 38/26: with niobium or tantalum
- C22C 38/40: with nickel
- C22C 38/42: with copper
- C22C 38/44: with molybdenum or tungsten
- C22C 38/48: with niobium or tantalum
- C23C 8/22: of ferrous surfaces
- C23C 8/54: Carbo-nitriding
- B22F 1/05: Metallic powder characterised by the size or surface area of the particles
- B22F 9/082: {atomising using a fluid (using centrifugal force B22F9/10)}
- B22F 2003/241: {Chemical after-treatment on the surface}
- B22F 2003/248: {Thermal after-treatment}
- B22F 2201/02: Nitrogen
- B22F 2201/30: Carburising atmosphere
- B22F 2998/10: Processes characterised by the sequence of their steps
- B22F 2999/00: Aspects linked to processes or compositions used in powder metallurgy
- C22C 33/0278: {with at least one alloying element having a minimum content above 5%}
- Y02P 10/25: Process efficiency
- C21D: MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING (surface treatment of metallic material involving at least one process provided for in class C23 and at least one process covered by this subclass C23F17/00; unidirectional solidification of eutectic materials or unidirectional demixing of eutectoid materials C30B)
- B22F: WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER (making alloys by powder metallurgy C22C); APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B23K: SOLDERING OR UNSOLDERING; WELDING; CLADDING OR PLATING BY SOLDERING OR WELDING; CUTTING BY APPLYING HEAT LOCALLY, e.g. FLAME CUTTING; WORKING BY LASER BEAM
- B33Y: ADDITIVE MANUFACTURING, i.e. MANUFACTURING OF THREE-DIMENSIONAL [3D] OBJECTS BY ADDITIVE DEPOSITION, ADDITIVE AGGLOMERATION OR ADDITIVE LAYERING, e.g. BY 3D PRINTING, STEREOLITHOGRAPHY OR SELECTIVE LASER SINTERING
- C22C: ALLOYS (treatment of alloys C21D, C22F)
- C23C: COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL (making metal-coated products by extrusion B21C23/22; covering with metal by connecting pre-existing layers to articles, see the relevant places, e.g. B21D39/00, B23K; metallising of glass C03C; metallising mortars, concrete, artificial stone, ceramics or natural stone C04B41/00; enamelling of, or applying a vitreous layer to, metals C23D; treating metal surfaces or coating of metals by electrolysis or electrophoresis C25D; single-crystal film growth C30B; by metallising textiles D06M11/83; decorating textiles by locally metallising D06Q1/04)
- Y02P: CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS

## Abstract

The present invention relates to alloy compositions for 3D metal printing procedures which provide metallic parts with high hardness, tensile strengths, yield strengths, and elongation. The alloys include Fe, Cr and Mo and at least three or more elements selected from C, Ni, Cu, Nb, Si and N. Ni may be replaced with Mn. As built parts indicate a tensile strength of at least 1000 MPa, yield strength of at least 640 MPa, elongation of at least 3.0% and hardness (HV) of at least 375.

## Claims

### Claim 1

A method of layer-by-layer construction of a metallic part comprising:
supplying particles of an iron-based alloy, the iron-based alloy comprising:
Fe in an amount ranging from 82.0 to 86.0 wt. %;
Cr in an amount ranging from 10.5 to 12.0 wt. %;
Mn in an amount ranging from 1.5 to 2.5 wt. %;
Mo in an amount ranging from 0.8 to 1.1 wt. %;
C in an amount ranging from 0.14 to 0.19 wt. %;
Nb in an amount ranging from 0.02 to 0.06 wt. %;
N in an amount ranging from 0.04 to 0.09 wt. %;
Si in an amount ranging from 0.25 wt. to 0.75 wt. %;
and
forming an as-built metallic part by powder bed fusing, said powder bed fusing comprising melting the particles into a molten state and cooling and forming one or more a solidified layers of the iron-based alloy
each of the one or more solidified layers has an as-formed thickness of 2.0 microns to 200.0 microns; and
said as-built metallic part has a tensile strength of at least 1000 MPa, a yield strength of at least 640 MPa, an elongation of at least 3.0%, and a hardness (HV) of at least 375.

### Claim 2 (depends on 1)

The method of claim 1, wherein said as-built metallic part has a tensile strength of 1000 MPa to 1900 MPa, a yield strength of 640 MPa to 1500 MPa, an elongation of 3.0% to 25.0%, and a hardness (HV) of 375 to 600.

### Claim 3 (depends on 1)

The method of claim 1, wherein each of said one or more layers has a thickness of 5.0 microns to 20.0 microns.

### Claim 4 (depends on 1)

The method of claim 1, wherein melting the particles is performed with one or more laser or electron beams with an energy density in the range of 30 J/mm3 to 500 J/mm3.

### Claim 5 (depends on 1)

The method of claim 1, wherein forming the as-built metallic part is performed in a nitrogen and/or argon atmosphere.

### Claim 6 (depends on 1)

The method of claim 1, wherein forming said as-built metallic part comprises forming said one or more solidified layers on a substrate that is preheated to a temperature of less than or equal to 300° C.

### Claim 7 (depends on 1)

The method of claim 1, further comprising heating the as-built metallic part at a temperature of greater than 900° C. followed by a gas quench and cooling to form a solutionized metallic part.

### Claim 8 (depends on 7)

The method of claim 7, further comprising tempering the solutionized metallic part at a temperature at or above 150° C. to form a tempered metallic part.

### Claim 9 (depends on 8)

The method of claim 8, wherein said tempered metallic part has a tensile strength of at least 1000 MPa, a yield strength of at least 900 MPa, an elongation of at least 1.0% and a hardness (HV) of at least 475.

### Claim 10 (depends on 8)

The method of claim 8, wherein the tempered metallic part has a surface, and the method further comprises carburizing the tempered metallic part to increase a level of carbon from the surface down to a depth of 4.0 mm.

### Claim 11 (depends on 8)

The method of claim 8, wherein the tempered metallic part has a surface, and the method further comprises nitriding the tempered metallic part to increase a level of nitrogen from the surface down to a depth of 400 μm.

### Claim 12 (depends on 1)

The method of claim 1, wherein said iron-based alloy comprises at least 0.88 wt. % Ni.

### Claim 13 (depends on 1)

The method of claim 1, wherein said iron-based alloy comprises at least 0.12 wt. % Cu.

### Claim 14 (depends on 1)

The method of claim 1, wherein said iron-based alloy comprises at least 0.03 wt. % Nb.

### Claim 15 (depends on 1)

The method of claim 1, wherein said iron-based alloy comprises at least 0.074 weight % N.

### Claim 16 (depends on 1)

The method of claim 1, wherein said iron-based alloy further comprises up to 1.0 wt. % of inevitable impurities.

### Claim 17 (depends on 3)

The method of claim 3, wherein the as-built metallic part is crack free.